Low-cost efficient flame-retardant PET floor and preparation method thereof

By using a combination of calcium carbonate and phosphorus-based flame retardant in PET floors, the flammability and droplet problems of PET floors are solved, and the low-cost and efficient flame retardant effect is achieved, meeting environmental protection and health requirements.

CN119039742APending Publication Date: 2024-11-29CHANGZHOU XINOU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411275489.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

PET floors are flammable and produce molten droplets when burning. The existing flame retardants have poor compatibility or produce harmful gases, which is difficult to meet environmental protection and health requirements.

Method used

A combination of a large amount of calcium carbonate and phosphorus-based flame retardant is used. Calcium carbonate is used as an inorganic filler to block the PET molecular chain group. The phosphorus-based flame retardant produces phosphoric acid and polyphosphate mucosal layer to prevent heat from spreading, and is used in combination to improve the flame retardant effect. Reduce costs.

Benefits of technology

It significantly improves the flame retardant effect of PET floors, reduces the cost and the amount of flame retardant, achieves a low-cost and efficient flame retardant effect, and reduces the generation of flue gas and harmful gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039742A_ABST
    Figure CN119039742A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of PET floors, and particularly discloses a low-cost efficient flame-retardant PET floor and a preparation method thereof. The low-cost efficient flame-retardant PET floor comprises the following raw materials in parts by weight: 100 parts of PET; 200 to 330 parts of calcium carbonate; 7-12 parts of a stabilizer; 1-5 parts of an internal lubricant; 1-5 parts of an external lubricant; 2-10 parts of a phosphorus-based flame retardant; the preparation method comprises the following steps: S1, mixing materials; s2, feeding the materials; s3, plasticizing is carried out; and S4, extruding. The PET floor can be used for floor laying of residences, office buildings and the like and has the advantages of being low in cost and high in flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of PET flooring, and more specifically, to a low-cost, high-efficiency, flame-retardant PET flooring and a preparation method thereof. Background Art

[0002] PET (polyethylene terephthalate) floor is a new type of non-toxic and environmentally friendly floor. In response to the increasingly stringent environmental protection requirements in the domestic and foreign markets, the PET environmentally friendly floor industry has developed rapidly. PET has excellent mechanical properties, chemical corrosion resistance, and dimensional stability at high temperatures. It is mainly used in plastic packaging bottles, films, synthetic fibers, electronic components, auto parts and other fields.

[0003] Since the limiting oxygen index of PET is only 20%-22%, it is a flammable polyester and it is easy to produce droplets when burning. Therefore, it is necessary to modify the conventional PET floor to be flame retardant. The flame retardants currently available on the market for PET products are generally divided into halogen, nitrogen, phosphorus and inorganic metal salts. Halogen flame retardants produce harmful gases such as dioxins and hydrogen halides during thermal decomposition, while nitrogen and inorganic metal salts have poor compatibility with PET resins. As people pay more attention to the ecological environment and physical health, it is urgent to develop a new type of PET flame retardant floor. Summary of the invention

[0004] In order to improve the flame retardant effect of the PET base plate, the present application provides a low-cost, high-efficiency, flame-retardant PET floor, which adopts the following technical solution:

[0005] In a first aspect, the present application provides a low-cost, high-efficiency, flame-retardant PET floor, comprising the following raw materials in parts by weight:

[0006] PET 100 parts;

[0007] Calcium carbonate 200-330 parts;

[0008] 7-12 parts of stabilizer;

[0009] Internal lubricant 1-5 parts;

[0010] 1-5 parts of external lubricant;

[0011] 2-10 parts of phosphorus flame retardant.

[0012] By adopting the above technical scheme, firstly, a large amount of calcium carbonate is introduced into the PET floor, and the addition of a large amount of inorganic fillers can effectively block the connection between the PET molecular chain groups, and then can block the transfer of heat and the activity of free radicals during combustion. It can also prevent the PET floor from producing droplets during the combustion process, and can effectively improve the flame retardant effect of the PET floor. Secondly, since the phosphorus-based flame retardant has the excellent characteristics of less smoke, low toxicity and high binding, it can produce a mucous film layer of phosphoric acid and polyphosphoric acid during combustion, which prevents the spread of heat and the spread of combustion. The generated inert gas can dilute the concentration of oxygen and combustible gas to achieve the purpose of flame retardancy. The combination of a large amount of calcium carbonate and phosphorus-based flame retardants can effectively improve the flame retardant effect of the PET floor, and can effectively reduce the cost of the PET floor and the amount of flame retardant, so that the PET floor obtains a low-cost, high-efficiency flame retardant effect.

[0013] Optionally, the stabilizer includes a calcium zinc stabilizer or a rare earth stabilizer.

[0014] Optionally, the internal lubricant includes any one of liquid paraffin, polyethylene wax and low molecular weight polypropylene.

[0015] Optionally, the external lubricant includes stearic acid or butyl stearate.

[0016] Optionally, the phosphorus-based flame retardant includes any one of organic hypophosphorous acid, organic hypophosphite compounds and phosphorus oxide.

[0017] In the second aspect, the present application provides a method for preparing a low-cost, high-efficiency, flame-retardant PET floor, using the following technical solution:

[0018] A method for preparing a low-cost, high-efficiency, flame-retardant PET floor comprises the following steps:

[0019] S1, mixing: take calcium carbonate, 2 / 3 weight part of PET, stabilizer, internal lubricant, external lubricant, phosphorus flame retardant, and remaining 1 / 3 weight part of PET respectively by weight, add materials in sequence, mix and discharge them into a cold mixing tank, cold mix, and obtain a mixture;

[0020] S2, feeding: transfer the mixed material to the extruder for preheating to obtain the preheated material. The first section barrel temperature of the extruder is 260-280°C, and the second section barrel temperature of the extruder is 250-270°C;

[0021] S3, plasticizing: convey the preheated material to the third and fourth sections of the extruder barrel for plasticizing to obtain plasticized material. During the plasticizing process, the pressure is maintained at 0.07-0.09MPa, the barrel temperature of the third section is 240-260°C, and the barrel temperature of the fourth section is 240-260°C;

[0022] S4, extrusion: convey the plasticized material to the fifth and sixth sections of the extruder barrel for mixing and merging, and extrude it into the molding die through the merging core to obtain the floor; the barrel temperature of the fifth section of the extruder barrel is 235-255°C, the barrel temperature of the sixth section of the extruder barrel is 235-255°C, and the temperature of the merging core is 235-255°C.

[0023] In summary, this application has the following beneficial effects:

[0024] 1. Since the present application introduces a large amount of calcium carbonate into the PET floor, the addition of a large amount of inorganic fillers can effectively block the connection between the PET molecular chain groups, thereby blocking the heat transfer and the activity of free radicals during combustion. It can also prevent the PET floor from generating droplets during the combustion process, and can effectively improve the flame retardant effect of the PET floor.

[0025] 2. In this application, since phosphorus-based flame retardant polymers have the excellent characteristics of less smoke, low toxicity and high bonding, they can produce a mucous layer of phosphoric acid and polyphosphoric acid during combustion to prevent the spread of heat and block the spread of combustion. The inert gas produced can dilute the concentration of oxygen and combustible gases to achieve the purpose of flame retardancy.

[0026] 3. In this application, by combining a large amount of calcium carbonate with phosphorus-based flame retardants, the flame retardant effect of the PET floor can be effectively improved, and the cost of the PET floor and the amount of flame retardant used can be effectively reduced, so that the PET floor achieves a low-cost, high-efficiency flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a flow chart of the method provided by this application. DETAILED DESCRIPTION

[0028] The present application is further described in detail below with reference to the embodiments.

[0029] Example

[0030] Example 1

[0031] On the one hand, the present application provides a low-cost, high-efficiency, flame-retardant PET floor, comprising 100 kg PET, 200 kg calcium carbonate, 7 kg calcium zinc stabilizer, 3 kg internal lubricant, 3 kg external lubricant and 5 kg organic hypophosphorous acid (2-carboxyethylphenylphosphinic acid industrial grade).

[0032] Specifically, calcium carbonate is selected from 200-800 mesh, the internal lubricant is liquid paraffin (CP42 chlorinated paraffin), and the external lubricant is stearic acid (industrial grade). PET is DuPont standard grade PET from the United States.

[0033] On the other hand, the present application provides a method for preparing a low-cost, high-efficiency, flame-retardant PET floor, comprising the following steps:

[0034] S1, mixing: take calcium carbonate, 2 / 3 weight part of PET, stabilizer, internal lubricant, external lubricant, phosphorus flame retardant, and remaining 1 / 3 weight part of PET respectively by weight, add materials in sequence, mix to 120°C and then discharge to a cold mixing tank, cold mix until the material temperature reaches 40°C and stop mixing to obtain a mixed material;

[0035] S2, feeding: the mixed material is transferred to the extruder for preheating to obtain the preheated material. The barrel temperature of the first section of the extruder is 280°C, and the barrel temperature of the second section of the extruder is 270°C;

[0036] S3, plasticizing: convey the preheated material to the third and fourth sections of the extruder barrel for plasticizing to obtain plasticized material. During the plasticizing process, the pressure is maintained at 0.07-0.09 MPa, the barrel temperature of the third section is 260°C, and the barrel temperature of the fourth section is 260°C;

[0037] S4, extrusion: the plasticized material is conveyed to the fifth and sixth sections of the extruder barrel for mixing and merging, and extruded from the merging core into the molding die to obtain a floor with a thickness of 5 mm; the barrel temperature of the fifth section of the extruder barrel is 255°C, the barrel temperature of the sixth section of the extruder barrel is 255°C, and the temperature of the merging core is 255°C.

[0038] Example 2

[0039] On the one hand, the present application provides a low-cost, high-efficiency, flame-retardant PET floor, comprising 100 kg PET, 330 kg calcium carbonate, 7 kg calcium zinc stabilizer, 3 kg internal lubricant, 3 kg external lubricant and 5 kg organic hypophosphorous acid.

[0040] Specifically, the calcium carbonate is 200-800 mesh, the internal lubricant is liquid paraffin, and the external lubricant is stearic acid.

[0041] On the other hand, the present application provides a method for preparing a low-cost, high-efficiency, flame-retardant PET floor, comprising the following steps:

[0042] S1, mixing: take calcium carbonate, 2 / 3 weight part of PET, stabilizer, internal lubricant, external lubricant, phosphorus flame retardant, and remaining 1 / 3 weight part of PET respectively by weight, add materials in sequence, mix to 120°C and then discharge to a cold mixing tank, cold mix until the material temperature reaches 40°C and stop mixing to obtain a mixed material;

[0043] S2, feeding: the mixed material is transferred to the extruder for preheating to obtain the preheated material. The barrel temperature of the first section of the extruder is 280°C, and the barrel temperature of the second section of the extruder is 270°C;

[0044] S3, plasticizing: convey the preheated material to the third and fourth sections of the extruder barrel for plasticizing to obtain plasticized material. During the plasticizing process, the pressure is maintained at 0.07-0.09 MPa, the barrel temperature of the third section is 260°C, and the barrel temperature of the fourth section is 260°C;

[0045] S4, extrusion: the plasticized material is conveyed to the fifth and sixth sections of the extruder barrel for mixing and merging, and extruded from the merging core into the molding die to obtain a floor with a thickness of 5 mm; the barrel temperature of the fifth section of the extruder barrel is 255°C, the barrel temperature of the sixth section of the extruder barrel is 255°C, and the temperature of the merging core is 255°C.

[0046] Example 3

[0047] On the one hand, the present application provides a low-cost, high-efficiency, flame-retardant PET floor, comprising 100 kg PET, 200 kg calcium carbonate, 7 kg calcium zinc stabilizer, 3 kg internal lubricant, 3 kg external lubricant and 10 kg organic hypophosphorous acid.

[0048] Specifically, the calcium carbonate is 200-800 mesh, the internal lubricant is liquid paraffin, and the external lubricant is stearic acid.

[0049] On the other hand, the present application provides a method for preparing a low-cost, high-efficiency, flame-retardant PET floor, comprising the following steps:

[0050] S1, mixing: take calcium carbonate, 2 / 3 weight part of PET, stabilizer, internal lubricant, external lubricant, phosphorus flame retardant, and remaining 1 / 3 weight part of PET respectively by weight, add materials in sequence, mix to 120°C and then discharge to a cold mixing tank, cold mix until the material temperature reaches 40°C and stop mixing to obtain a mixed material;

[0051] S2, feeding: the mixed material is transferred to the extruder for preheating to obtain the preheated material. The barrel temperature of the first section of the extruder is 280°C, and the barrel temperature of the second section of the extruder is 270°C;

[0052] S3, plasticizing: convey the preheated material to the third and fourth sections of the extruder barrel for plasticizing to obtain plasticized material. During the plasticizing process, the pressure is maintained at 0.07-0.09 MPa, the barrel temperature of the third section is 260°C, and the barrel temperature of the fourth section is 260°C;

[0053] S4, extrusion: the plasticized material is conveyed to the fifth and sixth sections of the extruder barrel for mixing and merging, and extruded from the merging core into the molding die to obtain a floor with a thickness of 5 mm; the barrel temperature of the fifth section of the extruder barrel is 255°C, the barrel temperature of the sixth section of the extruder barrel is 255°C, and the temperature of the merging core is 255°C.

[0054] Performance testing

[0055] (1) Limiting oxygen index test: According to ASTM D2863-2000, LOI (Limiting oxygen index, the minimum percentage of oxygen required to maintain the combustion of the sample material in a nitrogen and oxygen mixture, used to characterize the flame retardant effect of the flame retardant) was measured using an HC-2 oxygen index meter (Nanjing Jiangning Analytical Instrument Factory). The sample size was 140 mm × 6 mm × 3 mm.

[0056] (2) Flame retardant performance test: The CZF-II vertical combustion instrument was used to conduct vertical combustion tests on PET specimens. The specimen size was 125.0 mm × 13.0 mm × 3.0 mm, and the test standard was GB / T2408-2008. The samples were graded according to their burning time and the ignition of absorbent cotton, namely V-0, V-1, V-2, and NR.

[0057] Table 1 Performance test

[0058]

[0059] Combining the performance test comparison in Table 2, we can find that:

[0060] 1. By comparing with Examples 1-3, it can be found that the PET floor prepared in Examples 1-3 has a higher limiting oxygen index and resistance to droplets. This shows that in this application, the combination of phosphorus flame retardants and inorganic fillers solves the problem of PET being flammable and prone to droplets. Phosphorus flame retardants achieve flame retardant effects through gas phase and condensation phase mechanisms. Calcium carbonate, as a filler, on the one hand cuts off the connection between the PET molecular chain groups, and on the other hand prevents combustion from producing droplets, thereby achieving a flame retardant effect. The combination of phosphorus flame retardants and inorganic fillers not only achieves a flame retardant effect efficiently, but the filling of calcium carbonate not only reduces costs, but also reduces the amount of flame retardants used, thereby achieving the purpose of efficient flame retardancy while reducing costs.

[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low-cost, high-efficiency, flame-retardant PET floor. It is characterized in that The invention comprises the following raw materials in parts by weight: PET 100 parts; Calcium carbonate 200-330 parts; 7-12 parts of stabilizer; Internal lubricant 1-5 parts; 1-5 parts of external lubricant; 2-10 parts of phosphorus flame retardant.

2. A low-cost, high-efficiency, flame-retardant PET floor according to claim 1, Features: The stabilizer includes a calcium zinc stabilizer or a rare earth stabilizer.

3. A low-cost, high-efficiency, flame-retardant PET floor according to claim 1, Features: The internal lubricant includes any one of liquid paraffin, polyethylene wax and low molecular weight polypropylene.

4. A low-cost, high-efficiency, flame-retardant PET floor according to claim 1, Features: The external lubricant includes stearic acid or butyl stearate.

5. The low-cost, high-efficiency, flame-retardant PET floor according to claim 1, Features: The phosphorus-based flame retardant includes any one of organic hypophosphorous acid, organic hypophosphite compounds and phosphorus oxide.

6. A method for preparing a low-cost, high-efficiency, flame-retardant PET floor according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1, mixing: take calcium carbonate, 2 / 3 weight part of PET, stabilizer, internal lubricant, external lubricant, phosphorus flame retardant, and remaining 1 / 3 weight part of PET respectively by weight, add materials in sequence, mix and discharge them into a cold mixing tank, cold mix, and obtain a mixture; S2, feeding: transfer the mixed material to the extruder for preheating to obtain the preheated material. The first section barrel temperature of the extruder is 260-280°C, and the second section barrel temperature of the extruder is 250-270°C; S3, plasticizing: convey the preheated material to the third and fourth sections of the extruder barrel for plasticizing to obtain plasticized material. During the plasticizing process, the pressure is maintained at 0.07-0.09MPa, the barrel temperature of the third section is 240-260°C, and the barrel temperature of the fourth section is 240-260°C; S4, extrusion: convey the plasticized material to the fifth and sixth sections of the extruder barrel for mixing and merging, and extrude it into the molding die through the merging core to obtain the floor; the barrel temperature of the fifth section of the extruder barrel is 235-255°C, the barrel temperature of the sixth section of the extruder barrel is 235-255°C, and the temperature of the merging core is 235-255°C.