Glass or PET surface self-cleaning super-hydrophobic coating and preparation method thereof

By preparing a combined coating of sulfolactone acrylamide and epoxy resin on glass or PET surface, the existing coatings have been solved, and the weather resistance and light transmission are poor, achieving efficient self-cleaning and stability are reduced, and the environment and Health effects.

CN119039847AInactive Publication Date: 2024-11-29NANJING UNIV +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411292568.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing superhydrophobic coatings have problems such as poor weather resistance and light transmission, high fluorine content affects the environment and health, and low adhesion on the glass or PET surface, making it difficult to achieve efficient self-cleaning and stability.

Method used

Thiolactone acrylamide was prepared by extraction method of DL-homocysteine ​​sulfolide hydrochloride with NaHCO3, acryloyl chloride, saturated sodium chloride solution and ethyl acetate, followed by 1H,1H,2H,2H-full Fluorodecyl acrylate is crosslinked with a photoinitiator, and reaction is added with 4,4'-diaminodiphenyl methane and γ-glycidyl ether oxysilpropylsesquioxane to form an epoxy resin coating and pass through UV Light-induced and light-proof treatments ultimately cure at low and high temperatures.

Benefits of technology

The obtained coating has low surface energy, good UV resistance, self-cleaning effect and durability, which improves light transmittance and adhesion and reduces environmental and health impacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039847A_ABST
    Figure CN119039847A_ABST
Patent Text Reader

Abstract

The invention discloses a glass or PET surface self-cleaning super-hydrophobic coating and a preparation method thereof, and belongs to the technical field of self-cleaning materials. The method comprises the following steps: dissolving TlaAm in acetone powder, adding 1H, 1H, 2H, 2H-perfluorodecyl acrylate and a 184 photoinitiator, and irradiating and stirring through an ultraviolet lamp to obtain a precursor TTFP solution; dADCM is dissolved in tetrahydrofuran, a TTFP solution and DBU are added, stirring is carried out after light shielding treatment, GPOSS is added, stirring continues to be carried out, and a coating material is obtained; and coating the coating material on the surface of a base material, and heating and curing to obtain the glass or PET surface self-cleaning super-hydrophobic coating. The self-cleaning super-hydrophobic coating disclosed by the invention has low surface energy, the product shows good anti-ultraviolet performance through an inorganic siloxane inner core by utilizing an ultraviolet visible absorption spectrum, the product shows good low surface energy by utilizing a self-cleaning test, and the product shows good durability by utilizing a high-speed water flow test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of self-cleaning materials, and more particularly to a self-cleaning super-hydrophobic coating on a glass or PET surface and a preparation method thereof. Background Art

[0002] With the depletion of energy and the environmental crisis, the solar energy industry has emerged. For solar cells, in order to improve mechanical stability and serve as a barrier to pollutants, there is usually a glass cover, but after a long time, various pollutants such as dust will accumulate on the cover, which will affect the photoelectric conversion efficiency and thus reduce the efficiency of solar cells. By using super-hydrophobic coatings, we can achieve self-cleaning of glass surface pollution.

[0003] For super-hydrophobic coatings, their surface adhesion and friction coefficient are low, so the interface area between the polluted particles and the surface is very small, resulting in reduced adhesion. When water droplets fall on the coating, the pollution can easily roll off the surface with the water droplets, thus achieving self-cleaning.

[0004] Chinese invention patent CN115785761B discloses a method for preparing a fluorinated epoxy resin coating and a fluorinated epoxy resin coating. The method specifically includes: first preparing a fluorinated thiolactone prepolymer with a branched fluorinated alkane chain, and uniformly dispersing it with an amine curing agent and an epoxy resin to obtain a fluorinated epoxy resin coating solution. The prepared fluorinated epoxy resin coating is sprayed or brushed on the surface of the substrate, and after natural drying, it is cured at 120°C for 2 hours to obtain a fluorinated epoxy antifouling coating. This type of traditional fluorinated epoxy resin coating can take into account the high firmness and liquid repellency of epoxy resin, but has the following disadvantages: poor weather resistance and light transmittance; high fluorine content affects the environment and health; low adhesion to the substrate; and chemicals with low surface tension will spontaneously migrate to the surface.

[0005] Therefore, how to improve the coating and develop a self-cleaning super-hydrophobic coating for glass or PET surface and a preparation method thereof are problems that technicians in this field urgently need to solve. Summary of the invention

[0006] In view of this, the present invention provides a self-cleaning super hydrophobic coating on a glass or PET surface and a preparation method thereof.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface comprises the following steps:

[0009] (1) adding DL-homocysteine ​​thiolactone hydrochloride to a NaHCO3 solution and stirring, then adding acryloyl chloride and continuing to stir, then adding a saturated sodium chloride solution and ethyl acetate for extraction, filtering to obtain an organic phase, drying the organic phase with MgSO4, and then recrystallizing by rotary evaporation to obtain thiolactone acrylamide (TlaAm);

[0010] (2) dissolving thiolactone acrylamide in acetone powder, adding 1H, 1H, 2H, 2H-perfluorodecyl acrylate and 184 photoinitiator, irradiating with ultraviolet light and stirring to obtain a precursor tri-(2,2,2-trifluoroethyl) phosphite (TTFP) solution;

[0011] (3) dissolving 4,4'-diaminodiphenylmethane (DADCM) in tetrahydrofuran, adding the precursor tri-(2,2,2-trifluoroethyl)phosphite solution obtained in step (2) and 1,8-diazabicycloundec-7-ene (DBU), stirring after light protection, adding γ-glycidyloxysilylpropylsesquioxane (GPOSS) after stirring, and continuing to stir to obtain a coating material;

[0012] (4) applying the coating material on the surface of the substrate, heating and curing, and obtaining the self-cleaning super hydrophobic coating on the glass or PET surface.

[0013] Furthermore, in step (1), the mass ratio of DL-homocysteine ​​thiolactone hydrochloride, NaHCO3 and acryloyl chloride is (5-8):(18-20):(6-10).

[0014] The beneficial effect of adopting the above further technical solution is that the yield of thiolactone acrylamide (TlaAm) is at a higher level.

[0015] Preferably, in step (1), the mass ratio of DL-homocysteine ​​thiolactone hydrochloride, NaHCO3 and acryloyl chloride is 7:8.3.

[0016] Furthermore, in step (1), the mass volume ratio of acryloyl chloride, MgSO4, saturated sodium chloride solution and ethyl acetate is (6-10) g:(10-30) g:100 mL:(100-200) mL.

[0017] Preferably, in step (1), the mass volume ratio of acryloyl chloride, MgSO4, saturated sodium chloride solution and ethyl acetate is 8.3 g:30 g:100 mL:200 mL.

[0018] Furthermore, in step (1), after adding saturated sodium chloride solution and ethyl acetate for extraction, the operation of adding ethyl acetate is repeated and extraction is repeated twice.

[0019] The beneficial effects of adopting the above further technical solution are: making the extraction more complete and improving the purity of the organic phase obtained by extraction.

[0020] Furthermore, in step (1), the solvent of the NaHCO3 solution is water and 1,4-dioxane, the volume ratio of water to 1,4-dioxane is 1:1, and 18-20 g NaHCO3 is added to every 100 mL NaHCO3 solution.

[0021] Furthermore, in step (1), DL-homocysteine ​​thiolactone hydrochloride is added to a NaHCO3 solution and stirred at 0°C for 30 min at a stirring speed of 200 rpm, and then acryloyl chloride is added to the solution and stirred at room temperature for 30 min at a stirring speed of 200 rpm.

[0022] Furthermore, in step (2), the mass ratio of thiolactone acrylamide, acetone powder, 1H, 1H, 2H, 2H-perfluorodecyl acrylate and 184 photoinitiator is (1.8-2.2):(30-50):(2-3):(0.10-0.15).

[0023] The beneficial effect of adopting the above further technical solution is that the photoinitiated reaction proceeds relatively stably at this mass ratio, and the obtained cross-linking precursor tris-(2,2,2-trifluoroethyl)phosphite (TTFP) has a high purity.

[0024] Preferably, in step (2), the mass ratio of thiolactone acrylamide, acetone powder, 1H, 1H, 2H, 2H-perfluorodecyl acrylate and 184 photoinitiator is 2.0:40:2.18:0.15.

[0025] Furthermore, in step (2), the mixture was irradiated with a 400 W ultraviolet lamp, with a stirring speed of 200 rpm and a stirring time of 30 min.

[0026] Furthermore, in step (3), the mass ratio of 4,4'-diaminodiphenylmethane, tetrahydrofuran, tri-(2,2,2-trifluoroethyl)phosphite solution and 1,8-diazabicycloundec-7-ene is (0.5-0.6):(1.8-2):(0.24-0.48):(0.2-2.0), and the mass volume ratio of 1,8-diazabicycloundec-7-ene and γ-glycidyloxysilylpropylsesquioxane is (0.2-2.0) g:(4-5) μL.

[0027] The beneficial effect of adopting the above further technical solution is that at this ratio, the epoxy group can open smoothly and the thiolactone can open to form a thiol group.

[0028] Preferably, in step (3), the mass ratio of 4,4'-diaminodiphenylmethane, tetrahydrofuran, tris-(2,2,2-trifluoroethyl)phosphite solution and γ-glycidyloxysilylpropylsesquioxane is 0.58:2:0.32:1, and the mass volume ratio of 1,8-diazabicycloundec-7-ene and 1,8-diazabicycloundec-7-ene is 1 g:5 μL.

[0029] Furthermore, in step (3), the mixture is stirred for 30 minutes after the light-shielding treatment, and the stirring speed is 200 rpm; after stirring, γ-glycidyl ether silyl propyl sesquioxane is added and stirring is continued for 30 minutes, and the stirring speed is 200 rpm.

[0030] The beneficial effect of adopting the above further technical solution is that the reaction here is sensitive to light, and the reaction can be prevented from being affected by light and decomposition by avoiding light, and continuous stirring can make the reaction complete.

[0031] Furthermore, in step (4), the specific steps of heating and curing are: first curing at 70° C. for 30 minutes, and then curing at 90° C. for 30 minutes.

[0032] The beneficial effects of adopting the above-mentioned further technical solution are as follows: curing at 90°C is relatively complete, but long-term curing at high temperature will make the obtained coating yellow and reduce the transmittance. First curing to a certain extent at a relatively low 70°C and then switching to a relatively high 90°C curing can effectively avoid yellowing of the coating at long-term high temperature.

[0033] The present invention also provides a self-cleaning super-hydrophobic coating on the surface of glass or PET prepared by the method.

[0034] The inventive mechanism of the present invention:

[0035] 4,4'-diaminodiphenylmethane is dissolved in tetrahydrofuran, and the precursor tri-(2,2,2-trifluoroethyl)phosphite solution is added. The -NH2 in 4,4'-diaminodiphenylmethane causes the epoxy group to open the ring to obtain epoxy resin. The -NH2 in the added 4,4'-diaminodiphenylmethane induces the ring opening of thiolactone to generate thiol groups, and then 1,8-diazabicycloundec-7-ene crosslinking agent is added. The thiol groups can further react with γ-glycidyl ether silyl propyl sesquioxane and participate in the curing of epoxy.

[0036] The beneficial effects of the present invention are as follows: (1) The self-cleaning super hydrophobic coating on the glass or PET surface of the present invention has low surface energy. Through the inorganic siloxane core, using the ultraviolet visible absorption spectrum, the product shows good anti-ultraviolet performance. Using the self-cleaning test, the product shows good low surface energy. Using the high-speed water flow test, the product shows good durability.

[0037] (2) The reaction activity can be improved by introducing flexible organic substituents. The introduced fluoroalkane chain has a large polarity and can increase the intermolecular interaction, thereby enhancing the flexibility of the product and further improving the reaction activity.

[0038] (3) Trimethoxysilane can react with a hydroxyl-rich substrate to form a stable molecular layer. The thiol group participates in GPOSS bonding, which can improve the stability of the product. High-speed water flow testing can verify that the durability of the coating is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The present invention is a flow chart of steps (1) to (2) of the method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface;

[0040] Figure 2 Schematic diagram of -NH2-induced ring opening of epoxy groups to obtain epoxy resin;

[0041] Figure 3 Schematic diagram of -NH2-induced ring-opening of thiolactone to generate thiol groups, which can further react with γ-glycidyloxysilylpropylsesquioxane (GPOSS) for solidification;

[0042] Figure 4 This is a real picture of the self-cleaning super-hydrophobic coating on the glass surface of Example 1;

[0043] Figure 5 This is the UV spectrum of the transmittance of the self-cleaning super-hydrophobic coating on the glass surface of Example 1;

[0044] Figure 6 This is a physical picture of the self-cleaning effect of the self-cleaning super-hydrophobic coating on the glass surface of Example 1;

[0045] Figure 7 This is a bar chart of the durability test of the self-cleaning super-hydrophobic coating on the glass surface in Example 1. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] A method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface comprises the following steps:

[0049] (1) 7.0 g of DL-homocysteine ​​thiolactone hydrochloride was slowly added to 100 mL of NaHCO3 solution and stirred at 0°C for 30 min at a stirring speed of 200 rpm. The solvent of the NaHCO3 solution was water and 1,4-dioxane, and the volume ratio of water to 1,4-dioxane was 1:1. 19.15 g of NaHCO3 was added to 100 mL of NaHCO3 solution, and then 8.3 g of acryloyl chloride was added to the solution. The mixture was stirred at room temperature for 30 min at a stirring speed of 200 rpm. 100 mL of saturated sodium chloride solution and 200 mL of ethyl acetate were added for extraction. The ethyl acetate addition operation was repeated and the extraction was repeated twice. The organic phase was filtered to obtain the organic phase. The organic phase was dried with 30 g of MgSO4 and then recrystallized by rotary evaporation to obtain thiolactone acrylamide.

[0050] (2) Dissolve thiolactone acrylamide (2.01 g, 11.7 mmol) in 40 g of acetone powder, purify by filtering with a 0.22 μm syringe, add 1H, 1H, 2H, 2H-perfluorodecyl acrylate (5.18 g, 10 mmol) and 184 photoinitiator (0.15 g, 0.73 mmol), irradiate with a 400 W ultraviolet lamp and stir for 30 min at a stirring speed of 200 rpm to obtain a precursor tri-(2,2,2-trifluoroethyl) phosphite solution;

[0051] (3) 4,4'-diaminodiphenylmethane (0.58 g, 2.8 mmol) was dissolved in 2 g of tetrahydrofuran, and 0.32 g of the precursor tri-(2,2,2-trifluoroethyl)phosphite solution obtained in step (2) and 5 μL of 1,8-diazabicycloundec-7-ene were added, and the mixture was covered with aluminum foil to avoid light and stirred for 30 min at a stirring speed of 200 rpm. After stirring, 1 g of γ-glycidyl ether silyl propyl sesquioxane was added and stirring was continued for 30 min at a stirring speed of 200 rpm to obtain a coating material;

[0052] (4) Apply the coating material on the glass or PET surface, put it into the furnace for heating and curing, first cure it at 70°C for 30 minutes, and then cure it at 90°C for 30 minutes to obtain a self-cleaning super hydrophobic coating on the glass surface. Figure 4 .

[0053] Example 2

[0054] A method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface comprises the following steps:

[0055] (1) 6.0 g of DL-homocysteine ​​thiolactone hydrochloride was slowly added to 100 mL of NaHCO3 solution and stirred at 0°C for 30 min at a stirring speed of 200 rpm. The solvent of the NaHCO3 solution was water and 1,4-dioxane, and the volume ratio of water to 1,4-dioxane was 1:1. 18 g of NaHCO3 was added to 100 mL of NaHCO3 solution, and then 6 g of acryloyl chloride was added to the solution. The mixture was stirred at room temperature for 30 min at a stirring speed of 200 rpm. 100 mL of saturated sodium chloride solution and 200 mL of ethyl acetate were added for extraction. The operation of adding ethyl acetate was repeated, and the extraction was repeated twice. The organic phase was filtered to obtain the organic phase. The organic phase was dried with 30 g of MgSO4 and then recrystallized by rotary evaporation to obtain thiolactone acrylamide.

[0056] (2) Dissolve thiolactone acrylamide (2.01 g, 11.7 mmol) in 40 g of acetone powder, purify by filtering with a 0.22 μm syringe, add 1H, 1H, 2H, 2H-perfluorodecyl acrylate (5.18 g, 10 mmol) and 184 photoinitiator (0.15 g, 0.73 mmol), irradiate with a 400 W ultraviolet lamp and stir for 30 min at a stirring speed of 200 rpm to obtain a precursor tri-(2,2,2-trifluoroethyl) phosphite solution;

[0057] (3) 4,4'-diaminodiphenylmethane (0.58 g, 2.8 mmol) was dissolved in 1.8 g of tetrahydrofuran, and 0.24 g of the precursor tri-(2,2,2-trifluoroethyl)phosphite solution obtained in step (2) and 4 μL of 1,8-diazabicycloundec-7-ene were added, and the mixture was covered with aluminum foil to avoid light and stirred for 30 min at a stirring speed of 200 rpm. After stirring, 0.6 g of γ-glycidyl ether silyl propyl sesquioxane was added and stirring was continued for 30 min at a stirring speed of 200 rpm to obtain a coating material;

[0058] (4) The coating material is applied on the surface of glass or PET, and placed in a furnace for heating and curing, first at 70° C. for 30 min, and then at 90° C. for 30 min, to obtain a self-cleaning super hydrophobic coating on the surface of the glass or PET.

[0059] Example 3

[0060] A method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface comprises the following steps:

[0061] (1) 8 g of DL-homocysteine ​​thiolactone hydrochloride was slowly added to 100 mL of NaHCO3 solution and stirred at 0°C for 30 min at a stirring speed of 200 rpm. The solvent of the NaHCO3 solution was water and 1,4-dioxane, and the volume ratio of water to 1,4-dioxane was 1:1. 20 g of NaHCO3 was added to 100 mL of NaHCO3 solution, and then 10 g of acryloyl chloride was added to the solution. The mixture was stirred at room temperature for 30 min at a stirring speed of 200 rpm. 100 mL of saturated sodium chloride solution and 200 mL of ethyl acetate were added for extraction. The operation of adding ethyl acetate was repeated, and the extraction was repeated twice. The organic phase was filtered to obtain the organic phase. The organic phase was dried with 30 g of MgSO4 and then recrystallized by rotary evaporation to obtain thiolactone acrylamide.

[0062] (2) Dissolve thiolactone acrylamide (2.01 g, 11.7 mmol) in 40 g of acetone powder, purify by filtering with a 0.22 μm syringe, add 1H, 1H, 2H, 2H-perfluorodecyl acrylate (5.18 g, 10 mmol) and 184 photoinitiator (0.15 g, 0.73 mmol), irradiate with a 400 W ultraviolet lamp and stir for 30 min at a stirring speed of 200 rpm to obtain a precursor tri-(2,2,2-trifluoroethyl) phosphite solution;

[0063] (3) 4,4'-diaminodiphenylmethane (0.58 g, 2.8 mmol) was dissolved in 2 g of tetrahydrofuran, 0.48 g of the precursor tri-(2,2,2-trifluoroethyl)phosphite solution obtained in step (2) and 5 μL of 1,8-diazabicycloundec-7-ene were added, the mixture was covered with aluminum foil to avoid light and stirred for 30 min at a stirring speed of 200 rpm, and after stirring, 1 g of γ-glycidyl ether silyl propyl sesquioxane was added and stirring was continued for 30 min at a stirring speed of 200 rpm to obtain a coating material;

[0064] (4) The coating material is applied on the surface of PET or PET, and placed in a furnace for heating and curing, first at 70°C for 30 min, and then at 90°C for 30 min, to obtain a self-cleaning super hydrophobic coating on the surface of glass or PET.

[0065] Comparative Example 1

[0066] The difference between Comparative Example 1 and Example 1 is that the amount of γ-glycidyl ether silyl propyl sesquioxane used in step (3) is 0.5 g, and the other steps and parameters are the same. The obtained coating has condensation phenomenon and the self-cleaning effect is greatly reduced.

[0067] Conclusion: When the ratio of the precursor tris-(2,2,2-trifluoroethyl)phosphite solution to γ-glycidyloxysilylpropylsesquioxane exceeds 0.64, condensation will occur. Too large a ratio will cause the product to solidify rapidly, affecting the performance of light transmittance.

[0068] The difference between Comparative Example 2 and Example 1 is that the amount of the precursor tris-(2,2,2-trifluoroethyl)phosphite solution used in step (3) is 0.48 g, and the other steps and parameters are the same.

[0069] Conclusion: As a supporting sample for the previous conclusion, when the ratio of the precursor tris-(2,2,2-trifluoroethyl)phosphite solution to γ-glycidyloxysilylpropylsesquioxane is less than 0.64, no condensation will occur.

[0070] Example 1 The light transmittance of the self-cleaning super hydrophobic coating applied to glass and PET surfaces is shown in Figure 5 The ultraviolet spectrum of

[0071] Conclusion: After applying the coating designed by this method, it can be found that the light transmittance is improved to a certain extent, indicating that this method can achieve the effect of improving light transmittance.

[0072] Self-cleaning effect Figure 6 ;

[0073] Conclusion: When water drops pass through the coating surface inclined at 28°, they slide down and carry away the hydrophilic wool debris pollutants. After the entire self-cleaning process, all the pollutants on the coating surface are removed without any residual stains, and the self-cleaning effect is good.

[0074] Durability test see Figure 7 (From left to right, water flushing is 5 minutes, 10 minutes and 15 minutes).

[0075] Conclusion: After the test, the static contact angles of water and hexadecane changed slightly and were relatively stable. After the impact test, the coating still exhibited static hydrophobic and dynamic oleophobic properties.

[0076] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a self-cleaning super-hydrophobic coating on a glass or PET surface, characterized in that: The steps include: (1) adding DL-homocysteine ​​thiolactone hydrochloride to a NaHCO3 solution and stirring, then adding acryloyl chloride and continuing to stir, then adding a saturated sodium chloride solution and ethyl acetate for extraction, filtering to obtain an organic phase, drying the organic phase with MgSO4, and then recrystallizing by rotary evaporation to obtain thiolactone acrylamide; (2) dissolving thiolactone acrylamide in acetone powder, adding 1H, 1H, 2H, 2H-perfluorodecyl acrylate and 184 photoinitiator, irradiating with ultraviolet light and stirring to obtain a precursor tri-(2,2,2-trifluoroethyl) phosphite solution; (3) dissolving 4,4'-diaminodiphenylmethane in tetrahydrofuran, adding the precursor tri-(2,2,2-trifluoroethyl)phosphite solution and 1,8-diazabicycloundec-7-ene obtained in step (2), stirring after protecting from light, adding γ-glycidyl ether silyl propyl sesquioxane after stirring, and continuing to stir to obtain a coating material; (4) applying the coating material on the surface of the substrate, heating and curing, and obtaining the self-cleaning super hydrophobic coating on the glass or PET surface.

2. according to the preparation method of a kind of glass or PET surface self-cleaning super hydrophobic coating according to claim 1, it is characterized in that, In step (1), the mass ratio of DL-homocysteine ​​thiolactone hydrochloride, NaHCO3 and acryloyl chloride is (5-8):(18-20):(6-10).

3. according to the preparation method of a kind of glass or PET surface self-cleaning super hydrophobic coating according to claim 1, it is characterized in that, In step (1), the solvent of the NaHCO3 solution is water and 1,4-dioxane, the volume ratio of water to 1,4-dioxane is 1:1, and 18-20 g NaHCO3 is added to every 100 mL NaHCO3 solution.

4. according to the preparation method of a kind of glass or PET surface self-cleaning super hydrophobic coating according to claim 1, it is characterized in that, In step (1), DL-homocysteine ​​thiolactone hydrochloride is added to a NaHCO3 solution and stirred at 0°C for 30 min at a stirring speed of 200 rpm. Acryloyl chloride is then added to the solution and stirred at room temperature for 30 min at a stirring speed of 200 rpm.

5. according to the preparation method of a kind of glass or PET surface self-cleaning super hydrophobic coating according to claim 1, it is characterized in that, In step (2), the mass ratio of thiolactone acrylamide, acetone powder, 1H, 1H, 2H, 2H-perfluorodecyl acrylate and 184 photoinitiator is (1.8-2.2):(30-50):(2-3):(0.10-0.15).

6. A method for preparing a self-cleaning super-hydrophobic coating on glass or PET surface according to claim 1, characterized in that, In step (2), the mixture was irradiated with a 400 W ultraviolet lamp, with a stirring speed of 200 rpm and a stirring time of 30 min.

7. A method for preparing a self-cleaning super-hydrophobic coating on glass or PET surface according to claim 1, characterized in that, In step (3), the mass ratio of 4,4'-diaminodiphenylmethane, tetrahydrofuran, tris-(2,2,2-trifluoroethyl)phosphite solution and γ-glycidyl ether silyl propyl sesquioxane is (0.5-0.6):(1.8-2):(0.24-0.48):(0.2-2.0), and the mass volume ratio of γ-glycidyl ether silyl propyl sesquioxane and 1,8-diazabicycloundec-7-ene is (0.2-2.0) g:(4-5) μL.

8. A method for preparing a self-cleaning super-hydrophobic coating on glass or PET surface according to claim 1, characterized in that, In step (3), the mixture is stirred for 30 minutes after the light-shielding treatment, and the stirring speed is 200 rpm; after stirring, γ-glycidyl ether silyl propyl sesquioxane is added and stirring is continued for 30 minutes, and the stirring speed is 200 rpm.

9. A method for preparing a self-cleaning super-hydrophobic coating on glass or PET surface according to claim 1, characterized in that, In step (4), the specific steps of heating and curing are: first curing at 70°C for 30 minutes, and then curing at 90°C for 30 minutes.

10. A self-cleaning super hydrophobic coating on a glass or PET surface prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Hydrophobic and oleophobic modified epoxy resin as well as preparation method and application thereof

    CN119431737A

  • Preparation method of hydrophobic and oleophobic photovoltaic glass

    CN120398432A

  • A method for preparing hydrophobic and oleophobic photovoltaic glass

    CN120398432B