Method for preparing celsian fluorescent powder from Ba < 2 + >-doped zeolite material and application of celsian fluorescent powder

Through the low-temperature grinding and calcining process of Ba2+ doped zeolite materials, monoclinic barium feldspar phosphor with excellent performance was prepared, which solved the problems of high cost and poor stability of the existing barium feldspar phosphor preparation process, and achieved high efficiency and low The cost of barium feldspar phosphor preparation is suitable for white LED applications.

CN119039988APending Publication Date: 2024-11-29HEBEI UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411161601.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The preparation process of existing barium feldspar phosphor requires high temperature and high pressure, with high cost, low color rendering index and poor stability, making it difficult to meet the needs of low cost and simple processes.

Method used

Ba2+ doped zeolite material was used to prepare excellent monoclinic barium feldspar phosphors through low-temperature grinding and calcination, including reacting zeolite with BaCl2 solution, then mixing and grinding with EuCl3, and calcining in a presintering and reducing atmosphere to obtain BaSi2Al2O8 : xEu2+ barium feldspar phosphor.

Benefits of technology

The process of low-cost and low-temperature calcination is realized, which reduces the preparation cost, improves the quantum efficiency and thermal stability of the phosphor, solves the problems of low color rendering index and poor stability, and is suitable for the preparation of white LEDs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039988A_ABST
    Figure CN119039988A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing baryta feldspar fluorescent powder from a Ba < 2 + > doped zeolite material and application of the baryta feldspar fluorescent powder. The method comprises the following steps: taking Ba < 2 + > ion doped zeolite as a raw material, mixing with EuCl3, adding ethanol, performing wet grinding, presintering at 300-600 DEG C for 2-4 hours, and calcining at 600-900 DEG C in a reducing atmosphere to prepare the monoclinic celsian fluorescent powder with excellent performance. The obtained blue-light monoclinic celsian fluorescent powder has the characteristics of wide emission spectrum, high thermal stability and high quantum efficiency, a high-quality white light LED device is prepared from the blue-light monoclinic celsian fluorescent powder, and the problems of low color rendering index, poor stability and the like of a current commercial LED are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and particularly relates to a Ba 2+ A method for preparing celsium feldspar phosphor by doping zeolite material and its application in white light LED. Background Art

[0002] Baspar phosphors have attracted extensive attention from researchers due to their high quantum efficiency and good thermal stability. However, the preparation of monoclinic basalt requires high temperature, long reaction time and expensive alkoxides, which makes the phosphors face the defects of high preparation process cost and high cost. For example, the method proposed in patent CN202110810959.1 "A super-hydrophobic matrix material and preparation method of monoclinic basalt glass-ceramics" requires melting inorganic salts, which needs to be achieved at a high temperature of 1700°C. Patent CN201710101837.9 "Baspar phosphors have high thermal stability and high quantum efficiency, which requires high temperature and high cost. 2+ The method proposed in "Method for preparing barium feldspar bulk ceramics by replacing inorganic polymers" requires a high pressure of 1MPa and a long reaction time of 48 hours. Therefore, the development of a low-cost and simple preparation process is a key issue in the development of barium feldspar phosphors. Summary of the invention

[0003] The present invention aims to solve the problems of high reaction temperature, complex preparation process and expensive raw materials in the current preparation of barium feldspar phosphor. 2+ A method for preparing basite phosphor by doping zeolite material and its application. 2+ Ion-doped zeolite is used as a raw material, and after simple grinding, a monoclinic barium feldspar phosphor with excellent performance is prepared at a relatively low temperature. The blue light monoclinic barium feldspar phosphor obtained by the present invention has the characteristics of wide emission spectrum, strong thermal stability and high quantum efficiency. It is used to prepare high-quality white light LED devices, solving the problems of low color rendering index and poor stability faced by current commercial LEDs.

[0004] The present invention is achieved through the following technical solutions:

[0005] A kind of Ba 2+ A method for preparing celsium feldspar phosphor by doping zeolite material, the method comprising the following steps:

[0006] (1) adding zeolite to a BaCl2 solution, stirring under reflux at 60-90°C for 10-20 hours, washing and drying to obtain Ba-doped zeolite;

[0007] Wherein, 5 to 20 g of zeolite is added to every 200 mL of BaCl2 solution; the concentration of the BaCl2 solution is 0.01 to 1 M;

[0008] (2) Mix the Ba-doped zeolite obtained in step (1) with EuCl3, add ethanol and grind wetly for 1 to 3 hours to obtain the Eu 3+ -doped zeolite material;

[0009] wherein, the molar ratio is Ba:Eu = 1:0.1 to 0.3; 10 to 100 g of doped zeolite is added per 20 mL of ethanol;

[0010] (3) Pre-sinter the zeolite material prepared in step (2) at 300 to 600 °C for 2 to 4 hours; after cooling, the precursor of the celsian phosphor can be obtained;

[0011] (4) Put the precursor obtained in step (3) into a tube furnace, calcine at 600 to 900 °C for 1 to 3 hours in a reducing atmosphere, and after cooling, the celsian phosphor can be obtained.

[0012] The chemical formula of the celsian phosphor is BaSi2Al2O8:xEu 2+ ; wherein, x is the doping amount of Eu 2+ ions; 0.1 < x ≤ 0.3. The subscript is the celsian molecular formula, and x is the doping amount of Eu ions, that is, the ratio of Eu to Ba.

[0013] The zeolite material is SOD zeolite, A zeolite or faujasite.

[0014] The molar amount of Eu doping in the zeolite is 0.1 to 0.3 of the molar amount of Ba.

[0015] The reducing atmosphere is carbothermal reduction, carbon monoxide or hydrogen.

[0016] The application of the celsian phosphor prepared by the method is used to prepare white LED devices.

[0017] The beneficial effects of the present invention are as follows:

[0018] 1. The raw materials used are zeolites, which are simple to obtain, inexpensive, and have low cost.

[0019] 2. The preparation process is low-temperature calcination, which requires low equipment requirements and is easy to synthesize.

[0020] 3. The preparation method is ion exchange and grinding, which is easy for industrial production.

[0021] 4. The requirements for the type of zeolite are relatively low, including but not limited to A zeolite, SOD zeolite, faujasite, etc. Industrialized zeolites can be used, which can reduce the preparation cost of the phosphor by more than 50%.

[0022] 5. The requirements for the reducing atmosphere are low. It can be, but not limited to, various methods such as hydrogen reduction, carbothermal reduction, carbon monoxide reduction, etc., and can be flexibly adjusted according to production and industrial equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD spectrum of the celsium feldspar phosphor prepared from the SOD zeolite obtained in Examples 1 to 3.

[0024] Figure 2 This is the XRD spectrum of the celsium feldspar phosphor prepared from the A zeolite obtained in Examples 4 to 6.

[0025] Figure 3 This is the XRD spectrum of the celsium feldspar phosphor prepared from faujasite obtained in Examples 7 to 9.

[0026] Figure 4 The excitation and emission spectra of the celsium feldspar phosphor prepared from the SOD zeolite obtained in Examples 1 to 3.

[0027] Figure 5 The excitation and emission spectra of the celsium feldspar phosphor prepared from the A zeolite obtained in Examples 4 to 6.

[0028] Figure 6 These are the excitation and emission spectra of the celsium feldspar phosphor prepared from the faujasite zeolite obtained in Examples 7 to 9.

[0029] Figure 7 These are emission intensity spectra obtained in Examples 3, 6, and 9 at different temperatures.

[0030] Figure 8 Graph showing the emission spectra of the two white light LED devices obtained in Example 10. DETAILED DESCRIPTION

[0031] The following are non-limiting examples of the present invention.

[0032] Example 1: Preparation of barium feldspar phosphor by carbothermal reduction of SOD zeolite

[0033] (1) Weigh 10 g of SOD zeolite and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the "filtration, washing, drying" process three times to obtain BaCl2. 2+ Zeolite with complete ion exchange, wherein Na ions are completely exchanged with Ba ions in the zeolite during the ion exchange process, and then the excess impurity ions on the surface of the zeolite are washed away by washing.

[0034] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ion) obtained in step (1) and 0.015 mol of EuCl3, add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped SOD zeolite material.

[0035] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0036] (4) The precursor prepared in step (3) was placed in a tubular furnace and further calcined at 850°C for 2 hours in a carbon thermal reduction atmosphere (carbon monoxide is generated by the added carbon powder and a small amount of oxygen in the heating furnace under heating conditions, and then the sample is reduced). After cooling, ball milling was performed for 4 hours to obtain barium feldspar blue phosphor.

[0037] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 1 As shown in a. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which can prove that the crystal form of the phosphor is a monoclinic barium feldspar structure. During the ion exchange process of zeolite, Na ions are completely exchanged by Ba ions. The molecular formula of Ba-exchanged zeolite is BaSi2Al2O8. The calcination process changes the crystal form of zeolite, but does not change the elemental composition of zeolite. Eu ions are obtained by doping during the grinding process, and the chemical formula is BaSi2Al2O8:0.15Eu 2+ (theoretical value).

[0038] The excitation spectrum of the embodiment is as follows Figure 4 As shown in a in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 4 As shown in d, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications. At present, white light LEDs are generally composed of ultraviolet LED chips and three primary colors (red, green, and blue) phosphors. However, the "cyan defect" (480-500nm) between blue light and green light will make the color rendering index (CRI) of the prepared device lower. Therefore, preparing a broad-peak emission, especially a blue light phosphor with an emission range that includes cyan light, can effectively eliminate the cyan defect and improve the color rendering index of the prepared white light.

[0039] Example 2: Preparation of celsium feldspar phosphor in carbon monoxide reducing atmosphere SOD zeolite

[0040] (1) Weigh 10 g of SOD zeolite and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the "filtration, washing, drying" process three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0041] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped SOD zeolite material.

[0042] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0043] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 800° C. in a carbon monoxide reducing atmosphere for 2 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0044] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 1 As shown in b in the figure, the diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal structure is monoclinic barium feldspar.

[0045] The excitation spectrum of the embodiment is as follows Figure 4 As shown in curve b in the figure, the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region with a wavelength range of 250-400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 4 As shown in curve e in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0046] Example 3: Preparation of barium feldspar phosphor using SOD zeolite in hydrogen reduction atmosphere

[0047] (1) Weigh 10 g of SOD zeolite and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the "filtration, washing, drying" process three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0048] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped SOD zeolite material.

[0049] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0050] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 750° C. in a hydrogen reducing atmosphere for 2 hours. After cooling, the precursor was ball milled for 4 hours to obtain barium feldspar blue phosphor.

[0051] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 1 As shown in c in the figure. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal is a monoclinic barium feldspar structure.

[0052] The excitation spectrum of the embodiment is as follows Figure 4 As shown in curve c in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 4 As shown in curve f in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0053] Figure 7 Figure a tests the change in emission intensity of the phosphor prepared from SOD zeolite in the temperature range of 280–720K. When the temperature is 423K, the luminescence intensity of the phosphor can be maintained at more than 80% of that at room temperature, demonstrating its excellent thermal stability.

[0054] Example 4: Preparation of balsamite phosphor by carbothermal reduction of zeolite A

[0055] (1) Weigh 10 g of zeolite A and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0056] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain Eu-doped A zeolite material.

[0057] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0058] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 850° C. in a carbothermal reduction atmosphere for 1.5 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0059] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 2 As shown in a in the figure. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal is a monoclinic barium feldspar structure.

[0060] The excitation spectrum of the embodiment is as follows Figure 5 As shown in curve a in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 5 As shown in curve d in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, meaning that the phosphor has a good foundation in white light LED applications.

[0061] Example 5: Preparation of celsium feldspar phosphor in carbon monoxide reducing atmosphere A zeolite

[0062] (1) Weigh 10 g of zeolite A and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0063] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain Eu-doped A zeolite material.

[0064] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 3 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0065] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 800° C. in a carbon monoxide reducing atmosphere for 2 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0066] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 2 As shown in b in the figure, the diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal structure is monoclinic barium feldspar.

[0067] The excitation spectrum of the embodiment is as follows Figure 5 As shown in curve b in the figure, the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region with a wavelength range of 250-400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 5As shown in curve e in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0068] Example 6: Preparation of balsamite phosphor using zeolite A in hydrogen reduction atmosphere

[0069] (1) Weigh 10 g of zeolite A and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0070] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain Eu-doped A zeolite material.

[0071] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0072] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 750° C. in a hydrogen reducing atmosphere for 2 hours. After cooling, the precursor was ball milled for 4 hours to obtain barium feldspar blue phosphor.

[0073] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 2 As shown in c in the figure. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal is a monoclinic barium feldspar structure.

[0074] The excitation spectrum of the embodiment is as follows Figure 5 As shown in curve c in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 5 As shown in curve f in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0075] Figure 7 Figure b tests the change in emission intensity of the phosphor prepared from SOD zeolite in the temperature range of 280–720K. When the temperature is 423K, the luminescence intensity of the phosphor can be maintained at more than 80% of that at room temperature, demonstrating its excellent thermal stability.

[0076] Example 7: Preparation of barium feldspar phosphor from faujasite in carbothermal reduction atmosphere

[0077] (1) Weigh 10 g of faujasite and 200 mL (1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0078] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped faujasite material.

[0079] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0080] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 850° C. in a carbothermal reduction atmosphere for 2.5 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0081] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 3 As shown in a in the figure. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal structure is monoclinic barium feldspar.

[0082] The excitation spectrum of the embodiment is as follows Figure 6 As shown in curve a in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 6 As shown in curve d in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, meaning that the phosphor has a good foundation in white light LED applications.

[0083] Example 8: Preparation of barium feldspar phosphor using faujasite in a carbon monoxide reducing atmosphere

[0084] (1) Weigh 10 g of faujasite and 200 mL (0.1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0085] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped faujasite material.

[0086] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0087] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 800° C. in a carbon monoxide reducing atmosphere for 2.5 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0088] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 3 As shown in b in the figure, the diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal structure is monoclinic barium feldspar.

[0089] The excitation spectrum of the embodiment is as follows Figure 6 As shown in curve b in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 6 As shown in curve e in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0090] Example 9: Preparation of barium feldspar phosphor using faujasite zeolite in hydrogen reducing atmosphere

[0091] (1) Weigh 10 g of faujasite and 200 mL (0.1 M) BaCl2 solution into a round-bottom flask, reflux at 80 °C and stir for 24 hours, then repeat the process of "filtration, washing, and drying" three times to obtain BaCl2. 2+ A completely ion-exchanged zeolite.

[0092] (2) Weigh 37.5 g of the Ba-doped zeolite (0.1 mol of Ba ions) and 0.015 mol of EuCl3 obtained in step (1), add 20 mL of ethanol and wet grind for 3 hours to obtain the Eu-doped faujasite material.

[0093] (3) The zeolite material prepared in step (2) is placed in a muffle furnace and pre-sintered at 500° C. for 4 hours. After cooling, a barium feldspar blue phosphor precursor is obtained.

[0094] (4) The precursor prepared in step (3) was placed in a tube furnace and further calcined at 750° C. in a hydrogen reducing atmosphere for 2.5 hours. After cooling, the precursor was ball-milled for 4 hours to obtain barium feldspar blue phosphor.

[0095] In the embodiment of the present invention, the XRD diffraction pattern of the phosphor is as follows: Figure 3 As shown in c in the figure. The diffraction peak of the phosphor matches well with the monoclinic barium feldspar standard card, which proves that the phosphor crystal is a monoclinic barium feldspar structure.

[0096] The excitation spectrum of the embodiment is as follows Figure 6 As shown in curve c in FIG. 1 , the spectrum shows that the phosphor has a broad excitation peak in the near-ultraviolet region, with a wavelength range of 250 to 400 nm, which can be well matched with commercial near-ultraviolet chips. Figure 6 As shown in curve f in the figure, the spectrum shows that the emission peak of the phosphor is 400-600nm, with a peak value of 460nm, which is a broad-peak blue light emission, which means that the phosphor has a good foundation in white light LED applications.

[0097] Figure 7 Figure c in the figure tests the change of emission intensity of the phosphor prepared by SOD zeolite in the temperature range of ~720K. When the temperature is 423K, the luminescence intensity of the phosphor can be maintained at more than 80% of that at room temperature, proving its excellent thermal stability.

[0098] Example 10: Preparation of white light LED device

[0099] The present invention prepares two white light LED devices, including blue light celsium feldspar phosphor powder prepared by the present invention and yellow light Na6Si6Al6O 24 :Eu 2+ Phosphor, red phosphor is commercial red light Sr2Si5N8:Eu 2+ Phosphor(Ruixian Optical Materials, Sr2Si5N8:Eu 2+ The white light LED device prepared by using the commercial three-color phosphors (blue phosphor: Ruixian Optical Materials, BAM phosphor; green phosphor: Ruixian Optical Materials, S525 phosphor; red phosphor: Ruixian Optical Materials, Sr2Si5N8:Eu 2+ In addition, a fluorescence spectrometer is used to test the emission spectrum of the prepared white light LED device.

[0100] The UV chip used in the present invention is a commercial 365 UV chip, and there are no special requirements.

[0101] There is no special requirement for the amount of fluorescent powder used in the present invention, and it can be adjusted according to actual conditions.

[0102] Figure 8 It is an emission spectrum diagram of two prepared white light LED devices (the left one is the emission spectrum of the white light LED device prepared using commercial phosphors, and the right one is the emission spectrum of the white light LED device prepared using the phosphor of this patent). It can be seen from the figure that the white light emitted by the white light LED device prepared by the present invention has a lower correlated color temperature and a higher display index than the white light emitted by the current general commercial three-primary color phosphors, and exhibits a more excellent white light adjustment performance, which is obviously more advantageous in the application of commercial white light LEDs.

[0103] The above is only an example explanation of the present invention, and does not limit the specific implementation scheme. It is pointed out here that for those skilled in the art, without departing from the principle and protection scope of the present invention, the scheme can be further optimized, and the optimization can also be regarded as a protection for the preparation of barium feldspar phosphor by Ba ion-doped zeolite material and its application proposed in this scheme.

[0104] Matters not covered by the present invention are known technologies.

Claims

1. A kind of Ba 2+ The method for preparing celsium feldspar phosphor by doping zeolite material is characterized in that the method comprises the following steps: (1) adding zeolite to a BaCl2 solution, stirring under reflux at 60-90°C for 10-20 hours, washing and drying to obtain Ba-doped zeolite; Wherein, 5 to 20 g of zeolite is added to every 200 mL of BaCl2 solution; the concentration of the BaCl2 solution is 0.01 to 1 M; (2) The Ba-doped zeolite obtained in step (1) is mixed with EuCl3, and wet-ground with ethanol for 1 to 3 hours to obtain EuCl3. 3+ doped zeolite materials; The molar ratio is Ba:Eu=1:0.1-0.3; 10-100 g of doped zeolite is added to every 20 mL of ethanol; (3) pre-sintering the zeolite material prepared in step (2) at 300-600° C. for 2-4 hours; after cooling, a barium feldspar phosphor precursor can be obtained; (4) The precursor obtained in step (3) is placed in a tube furnace and calcined at 600-900° C. for 1-3 hours in a reducing atmosphere. After cooling, barium feldspar phosphor powder is obtained.

2. Ba as claimed in claim 1 2+ A method for preparing barium feldspar phosphor by doping zeolite material, characterized in that the chemical formula of the barium feldspar phosphor is BaSi2Al2O8:xEu 2+ ;in, x is Eu 2+ Ion doping amount; 0.1 <x≤0.3。 3. Ba as claimed in claim 1 2+ The invention discloses a method for preparing celsium feldspar phosphor by doping zeolite material, wherein the zeolite material is SOD zeolite, A zeolite or faujasite zeolite.

4. Ba as claimed in claim 1 2+ A method for preparing celsium feldspar phosphor by doping zeolite material, characterized in that The reducing atmosphere is carbothermal reduction, carbon monoxide or hydrogen.

5. Ba as claimed in claim 1 2+ The invention discloses a method for preparing barium feldspar phosphor by doping zeolite material, which is characterized by using the barium feldspar phosphor prepared by the method to prepare white light LED devices.

Citation Information

Patent Citations

  • Method for preparing barium feldspar blocky ceramics through inorganic polymer replacement by Ba&lt;2+&gt;

    CN106747382A

  • Super-hydrophobic matrix material of monoclinic-phase celsian glass ceramic and preparation method thereof

    CN113735449A