Composite current collector and preparation method thereof
By plating the Au layer in the composite liquid collector and using malachite green and ethylenediamine additives to regulate the crystal plane orientation of the copper layer, the problem of insufficient tensile strength and elongation of the composite liquid collector is solved, and the material is significantly improved electrical conductivity and mechanical properties.
Patent Information
- Application Number
- CN202411262364.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
The insufficient tensile strength and low elongation of the composite copper current collector lead to problems such as strip breakage during use, affecting battery performance.
By plating the copper layer on the base layer and using malachite green and ethylenediamine as additives on its surface, the Cu(200) crystal plane orientation is regulated, and the conductivity and mechanical properties of the copper layer are enhanced. Improve tensile strength and elongation.
It significantly improves the tensile strength and elongation of the composite fluid collection, reduces the resistivity, enhances the overall performance of the material, and solves the problem of insufficient tensile strength and elongation.
Smart Images

Figure CN119040832A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite current collectors, and specifically discloses a composite current collector and a preparation method thereof. Background Art
[0002] With the rapid development of new energy and electronic technology, the requirements for battery cycle life, safety performance, and energy density are getting higher and higher. As a very important part of the battery, the current collector is used to collect the current generated by the active material of the battery to form a larger current output. Its performance will directly affect the performance of the battery.
[0003] At present, copper foil and aluminum foil are mostly used as current collectors for positive and negative electrodes in lithium batteries and sodium batteries. This type of current collector is not conducive to controlling battery costs and improving energy density. In this regard, composite foil has obvious advantages over traditional foil. Composite foil current collectors are usually a "sandwich" structure, with a polymer high molecular layer as the inner layer and metal conductive layers on both sides. The metal layer on the surface of the composite current collector is thinner and the internal polymer layer is lighter, which can greatly reduce the overall weight of the current collector and thus increase the energy density of the lithium-ion battery; at the same time, the thinner metal layer on the surface of the composite current collector is easier to disconnect than the traditional foil current collector when the lithium-ion battery has thermal runaway, thereby isolating the connection between the active material and the current collector and preventing the lithium-ion battery from continuing to have thermal runaway.
[0004] Although composite foil has the advantages of low cost and light weight, the current composite copper current collector has the problems of insufficient tensile strength and low elongation, which causes a series of other problems such as broken foil in the subsequent use process. Therefore, improving the tensile strength and elongation of the composite current collector has become an important topic. In summary, it is of great significance to study a composite current collector with good tensile strength and good elongation and its preparation method. Summary of the invention
[0005] The object of the present invention is to provide a composite current collector and a preparation method thereof to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a composite current collector: comprising the following steps: S1: Equipment preparation: preparing a high vacuum winding magnetron sputtering device to ensure that the equipment operates normally; preparing a water plating line to ensure that it can operate normally; selecting a suitable Au as a target material, and performing surface treatment (mechanical grinding to remove uneven parts) to ensure that the surface of the target material is flat and free of impurities; taking a base film (1) as a base layer, and plating a gold layer on both sides by magnetron sputtering after plasma treatment to obtain a transition layer (2); S2: Plating the surface of the transition layer with water to obtain a copper layer (3) and a composite current collector; the water plating solution used in the water plating process specifically includes the following raw materials: 0.04-0.15 g / L additive, 80-140 g / L copper sulfate, 90-150 g / L sulfuric acid, 40-70 ppm chloride ion, 1-10 ml / L copper plating auxiliary agent, and the rest is water.
[0007] More optimally, the copper plating auxiliary agent includes 2~5ml / L of Jie Ruimei copper plating additive 200-A; 1~5ml / L of Jie Ruimei copper plating additive 200-B.
[0008] More optimally, the additive includes the following raw materials: 0.01-0.07 g / L malachite green and 0.03-0.08 g / L ethylenediamine.
[0009] More optimally, the thickness of the base layer is 4-6 μm; the thickness of the transition layer is 5%-10% of the thickness of the base layer; and the thickness of the copper layer is 0.5-1.5 μm.
[0010] More optimally, the specific process of water plating is: plating solution temperature 20°C~28°C, electroplating time 10~15min, current 3000A~5000A.
[0011] More optimally, the material of the base film includes one or more of polypropylene, non-isocyanate polyurethane acrylate monomer, methyl acrylate, vinyl acetate, n-butyl methacrylate, styrene, acrylonitrile, acrylamide, rosin resin, acrylate polymer, and terpene resin.
[0012] More optimally, the specific process of the magnetron sputtering is: setting the substrate temperature of the winding coating to 10~12°C, the sputtering target distance to 10~12cm, the target power to 13~15kw, and the argon gas flow rate to 50~55sccm.
[0013] More optimally, the plasma voltage of the plasma treatment is 500-550V.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention first plates Au layers (gold layers) on both sides of the substrate layer by magnetron sputtering, which has better conductivity; then plates the copper layer by water plating process, and the additive malachite green (MG) is added during water plating. Since the interaction between malachite green and the Cu (111) surface is stronger than that between malachite green and the Cu (200) surface, this stronger interaction partially prevents the epitaxial growth of the Cu (111) surface and promotes the further growth of the Cu (200) surface. Therefore, after being added as an additive, the growth of the copper layer in the water plating process can have a clear Cu (200) growth orientation, forming square pyramidal microcrystals in the Cu (200) direction; When electrons and other carriers move in a crystal, they encounter a grain boundary. The irregular arrangement of atoms at the grain boundary will cause the carrier's movement path to change and slow down. This scattering effect will increase the resistance to carrier movement, thereby affecting the electrical conductivity, thermal conductivity, tensile strength, etc. of the material. Therefore, the present invention adjusts the performance of the material by properly controlling the characteristics of the grain boundary, that is, by adding additives, the Cu (200) crystal plane orientation occupies the majority of the coating, and the surface energy of the grains with the consistent Cu (200) crystal plane orientation is relatively low, which helps to reduce the resistivity and improve the tensile strength. The addition of ethylenediamine (EDA) can refine the grains, strengthen the mechanical properties, and simultaneously improve the tensile strength and elongation. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 1 is a diagram of the composite current collector structure; wherein, number 1 in the figure is the base layer; number 2 in the figure is the transition layer; and number 3 in the figure is the metal layer. DETAILED DESCRIPTION
[0016] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0017] The following parts are by mass unless otherwise specified; Embodiment 1: S1: Equipment preparation: prepare a high vacuum winding magnetron sputtering equipment to ensure that the equipment operates normally; prepare a water plating line to ensure that it can operate normally; select Au as the target material, and perform surface treatment to ensure that the target surface is flat and free of impurities; take a 4.5 μm thick polypropylene film as the base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, set the base temperature of the winding coating to 10°C, the sputtering target distance to 10 cm, the target power to 13 kW, and the argon gas flow rate to 50 sccm for magnetron sputtering coating, obtain gold layers on both sides, and obtain a 50 nm thick transition layer; S2: water plating on the surface of the transition layer to obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 0.04g / L malachite green, 0.05g / L ethylenediamine, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0018] Comparative Example 1 (EDA is not added, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a high vacuum winding magnetron sputtering equipment to ensure that the equipment operates normally; prepare a water plating line to ensure that it can operate normally; select Au as the target material, and perform surface treatment to ensure that the surface of the target material is flat and free of impurities; take a 4.5 μm thick polypropylene film as the base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, set the base temperature of the winding coating to 10°C, the sputtering target distance to 10 cm, the target power to 13 kW, and the argon gas flow rate to 50 sccm for magnetron sputtering coating, and obtain gold layers on both sides to obtain a 50 nm thick transition layer; S2: water plating on the surface of the transition layer to obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 0.04g / L malachite green, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0019] Comparative Example 2 (MG is not added, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a high vacuum winding magnetron sputtering equipment to ensure that the equipment operates normally; prepare a water plating line to ensure that it can operate normally; select Au as the target material, and perform surface treatment to ensure that the surface of the target material is flat and free of impurities; take a 4.5 μm thick polypropylene film as the base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, set the base temperature of the winding coating to 10°C, the sputtering target distance to 10 cm, the target power to 13 kW, and the argon gas flow rate to 50 sccm for magnetron sputtering coating, and obtain gold layers on both sides to obtain a 50 nm thick transition layer; S2: water plating on the surface of the transition layer to obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 0.05g / L ethylenediamine, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, electroplating time 8min, current 3200A Comparative Example 3 (the magnetron sputtering target is ordinary copper, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a high vacuum winding magnetron sputtering equipment to ensure that the equipment operates normally; prepare a water plating line to ensure that it can operate normally; select copper as the target material, and perform surface treatment to ensure that the target surface is flat and free of impurities; take a 4.5 μm thick polypropylene film as the base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, set the base temperature of the winding coating to 10°C, the sputtering target distance to 10 cm, the target power to 13 kW, and the argon gas flow rate to 50 sccm for magnetron sputtering coating, and obtain gold layers on both sides to obtain a 50 nm thick transition layer; S2: water plating on the surface of the transition layer to obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 0.04g / L malachite green, 0.05g / L ethylenediamine, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0020] Comparative Example 4 (MG and EDA are not added, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a high vacuum winding magnetron sputtering equipment to ensure that the equipment operates normally; prepare a water plating line to ensure that it can operate normally; select Au as the target material, and perform surface treatment to ensure that the target surface is flat and free of impurities; take a 4.5 μm thick polypropylene film as the base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, set the base temperature of the winding coating to 10°C, the sputtering target distance to 10 cm, the target power to 13 kW, and the argon gas flow rate to 50 sccm for magnetron sputtering coating, and obtain gold layers on both sides to obtain a 50 nm thick transition layer; S2: water plating on the surface of the transition layer to obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0021] Comparative Example 5 (no transition layer, no EDA, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a water plating line to ensure that it can operate normally; take a 4.5 μm thick polypropylene film as a base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, perform water plating, and obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process specifically includes the following raw materials: 0.04g / L malachite green, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0022] Comparative Example 6 (no transition layer, no MG, and the remaining steps are consistent with Example 1): S1: Equipment preparation: prepare a water plating line to ensure that it can operate normally; take a 4.5 μm thick polypropylene film as a base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, perform water plating, and obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 0.05g / L ethylenediamine, 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0023] Comparative Example 7 (no transition layer, no EDA, no MG, and the remaining method steps are consistent with Example 1): S1: Equipment preparation: prepare a water plating line to ensure that it can operate normally; take a 4.5 μm thick polypropylene film as a base film to obtain a base layer, perform plasma treatment at a plasma voltage of 500 V, perform water plating, and obtain a 1 μm copper layer on both sides to obtain a composite current collector; The water plating solution used in the water plating process includes the following raw materials: 110g / L copper sulfate, 120g / L sulfuric acid, hydrochloric acid (chloride ion 60ppm), 4ml / L Jie Ruimei copper plating additive 200-A, 2ml / L Jie Ruimei copper plating additive 200-B, and the rest is water; The water plating process is: bath temperature 24°C, plating time 8min, current 3200A.
[0024] In the above examples, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: polypropylene film (Kaideli 6018H); malachite green (CAS: 569-64-2, Guangdong Xiaoda Chemical Industry); ethylenediamine (CAS: 109-89-7).
[0025] Experiment: Take the composite current collector prepared in Example 1 and Comparative Examples 1 to 7; (1) Tensile strength test after heat aging test at 120°C x 2min: Take the finished product prepared by the present invention as a sample, and use MTS Criterion42 tensile testing machine to measure the tensile strength of the film; Parameter setting: The clamp spacing on the tensile testing machine is 100mm, the test speed is (250±25)mm / min, and the tensile strength is obtained by testing; (2) Elongation at break test: Use MTS Criterion42 tensile testing machine to measure the elongation at break of the film. Parameter setting: The clamp spacing on the tensile testing machine is 100mm, and the test speed is (250±25)mm / min; the specific data is in the table below;
[0026] Conclusion: It can be seen from the above table that by plating Au layers on both sides of the substrate layer by magnetron sputtering and then plating a copper layer with the assistance of additives (malachite green + ethylenediamine), the properties of the grain boundaries can be regulated to adjust the performance of the material and improve the tensile strength and elongation; when the Au layer is not plated or the additive formula is changed, the performance will be reduced. In summary, the composite current collector prepared by the process of the present invention has good tensile properties and elongation.
[0027] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a composite current collector, characterized in that: The following steps are involved: S1: taking a base film (1) as a base layer, plating a gold layer on both sides by magnetron sputtering after plasma treatment to obtain a transition layer (2); S2: Plating the surface of the transition layer with water to obtain a copper layer (3) and a composite current collector; the water plating solution used in the water plating process specifically includes the following raw materials: 0.04-0.15 g / L additive, 80-140 g / L copper sulfate, 90-150 g / L sulfuric acid, 40-70 ppm chloride ion, 1-10 ml / L copper plating auxiliary agent, and the rest is water.
2. The method for preparing a composite current collector according to claim 1, characterized in that: The additive comprises the following raw materials: 0.01-0.07 g / L malachite green and 0.03-0.08 g / L ethylenediamine.
3. The method for preparing a composite current collector according to claim 1, characterized in that: The thickness of the base layer is 4-6 μm; the thickness of the transition layer is 5%-10% of the thickness of the base layer; and the thickness of the copper layer is 0.5-1.5 μm.
4. The method for preparing a composite current collector according to claim 1, characterized in that: The specific process of water plating is: plating solution temperature is 20°C~28°C, electroplating time is 10~15min, and current is 3000A~5000A.
5. The method for preparing a composite current collector according to claim 1, characterized in that: The material of the base film includes one or more of polypropylene, non-isocyanate polyurethane acrylate monomer, methyl acrylate, vinyl acetate, n-butyl methacrylate, styrene, acrylonitrile, acrylamide, rosin resin, acrylate polymer, and terpene resin.
6. The method for preparing a composite current collector according to claim 1, characterized in that: The specific process of the magnetron sputtering is as follows: setting the substrate temperature of the winding coating to 10-12°C, the sputtering target distance to 10-12cm, the target power to 13-15kw, and the argon gas flow rate to 50-55sccm.
7. The method for preparing a composite current collector according to claim 1, characterized in that: The plasma voltage of the plasma treatment is 500-550V.
8. A composite current collector prepared according to the method for preparing a composite current collector according to any one of claims 1 to 7.
Citation Information
Cited By
Functional current collector, pole piece using same and battery
CN119742372A
Preparation method and application of functional current collector with low thermal shrinkage and high tensile strength
CN119864424A
Preparation Method and Application of a Functional Current Collector with Low Thermal Shrinkage and High Tensile Strength