Flame-retardant polyvinyl chloride cable and preparation process thereof
By using the bilayer structure of materials such as N,N'-piperazine di(methylphosphoric acid), modified basalt and modified white mud in the cable, combined with silane coupling agent modified phytate and magnesium hydroxide , solve the problem of toxic gases in the prior art, and realize high flame retardant performance and environmentally friendly cable preparation.
Patent Information
- Application Number
- CN202411334644.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the use of flame retardant will produce toxic gases, which limits its application. In addition, polyvinyl chloride emits harmful gases during the flame retardant process, making it difficult to meet the needs of environmental protection and high flame retardant performance.
A flame retardant filler layer consisting of N,N'-piperazine di(methylphosphoric acid), modified basalt and modified white mud are used to form a double-layer flame retardant structure by introducing silane couples. Coupling agent-modified materials such as phytate and magnesium hydroxide improve the flame retardant performance of the cable.
The cable with high flame retardant performance has been achieved. Through the combination of a double-layer structure and a modified material, the flame retardant effect of the sheath is enhanced, the generation of harmful gases is reduced, and the dispersion and flame retardant performance of the material are improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cables and relates to a flame-retardant polyvinyl chloride cable and a preparation process thereof. Background Art
[0002] With the rapid development of the global economy and the enhancement of human environmental awareness, the requirements for the quality and performance of wires and cables in various fields are becoming higher and higher. In particular, the situation of fire caused by short circuit of wires has attracted particular attention. Therefore, how to improve the flame retardant performance of cables has also become the development direction of the wire and cable industry. At present, in order to improve the flame retardant performance of cables, people usually choose polyvinyl chloride or halogen-free low-smoke polyethylene as the main raw material for sheath tubes. However, although polyvinyl chloride can achieve a certain flame retardant effect, polyvinyl chloride will emit a large amount of harmful gas hydrogen chloride during the flame retardant process, while halogen-free low-smoke polyethylene will not produce harmful gases. Flame retardant polymer materials are mainly achieved by adding flame retardants and introducing flame retardant elements or groups.
[0003] Halogen flame retardants can release hydrogen halides during thermal decomposition, which react with high-energy free radicals generated by polymer combustion. The generated halogen free radicals can continue to participate in the reaction, and the combustion reaction is blocked in this cycle. At the same time, hydrogen halide gas can also effectively dilute oxygen to achieve the purpose of flame retardancy. However, combustion will produce toxic hydrogen halide gas, polybrominated benzooxins and polybrominated dibenzofurans and other carcinogens. Therefore, the application of halogen flame retardants is limited.
[0004] In view of the above problems, the present invention provides a flame retardant polyvinyl chloride cable and a preparation process thereof, which can effectively solve the above problems. Summary of the invention
[0005] The present invention relates to a flame-retardant polyvinyl chloride cable and a preparation process thereof, and belongs to the technical field of cables. The flame-retardant polyvinyl chloride cable disclosed in the present invention has a structure from inside to outside of a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, wherein the flame-retardant filling layer is composed of N, N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud, and the polyvinyl chloride composite sheath is composited with polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud. The present invention forms a double-layer flame-retardant structure through the flame-retardant filling layer and the polyvinyl chloride composite sheath, thereby obtaining a highly flame-retardant polyvinyl chloride cable.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A flame-retardant polyvinyl chloride cable, the structure of the flame-retardant polyvinyl chloride cable from inside to outside is a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, the flame-retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.1-0.3:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:1.
[0007] Furthermore, the preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add modified phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
[0008] Furthermore, in the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 80-100° C. and 2-3 h, respectively, and the drying temperature and time are 100-110° C. and 24 h, respectively.
[0009] Furthermore, in the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g: 0.1-0.2 g: 800-1000 mL, the temperature and time of the heating and stirring are 80° C. and 2-3 h, respectively, and the temperature and time of the drying are 100-110° C. and 24 h, respectively.
[0010] Furthermore, in the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:9-10g:800-1000mL, the temperature and time of heating and stirring are 80°C and 2-3h respectively, and the temperature and time of drying are 100-110°C and 24h respectively.
[0011] Furthermore, the preparation method of the modified phytate in step (3) is: mixing a silane coupling agent, phytate and ammonium polyphosphate in a mass ratio of 1:0.5-5:30-40, then heating and stirring, and cooling to obtain the modified phytate, wherein the phytate is calcium phytate, and the temperature and time of heating and stirring are 100-150°C and 1-2h respectively.
[0012] Furthermore, the preparation method of the modified white mud is: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
[0013] Furthermore, the temperature and time of the drying and grinding are 100-110°C and 24h respectively, the particle size of the white mud powder is 3-5μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50g:500-700mL:3g, and the temperature and time of the heating and stirring are 80°C and 5-6h respectively.
[0014] Furthermore, the preparation process of the flame-retardant polyvinyl chloride cable is as follows: the wire core and the flame-retardant filling layer are placed in a mold, and then formed and extruded with the polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 200-220°C, and the wire core is an aluminum wire.
[0015] Beneficial effects of the present invention: 1. By introducing phytate modified with silane coupling agent, it can be firmly deposited on the surface of basalt, making the modified basalt have good dispersibility. At the same time, the introduction of nickel and magnesium elements further improves the flame retardant effect; 2. Modified basalt has inorganic flame retardant and carbon-promoting effects, and decomposes with modified white mud and magnesium hydroxide with smoke suppression effect to form water vapor. The polyvinyl chloride composite sheath composed of the three enhances the flame retardant effect of the sheath from the dimensions of condensed phase, gas phase and heat absorption; 3. N,N'-piperazine di(methylphosphonic acid) in the flame-retardant filling layer can volatilize PO2·, PO· and HPO· free radicals in the gas phase, which inhibits H· and OH· free radicals. At the same time, the dehydration of phosphoric acid produced promotes carbonization, thereby preventing the combustion of the material. The flame-retardant filling forms a double-layer flame-retardant structure with the polyvinyl chloride composite sheath, thereby obtaining a highly flame-retardant polyvinyl chloride cable. DETAILED DESCRIPTION
[0016] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0017] In all embodiments and comparative examples of the present invention, N,N'-piperazine di(methylphosphonic acid) was purchased from: Henan Lien Chemical Products Co., Ltd. / 89280-71-7; basalt powder was purchased from: Chen Ming / specification 0.065 mm; the silane coupling agent was purchased from: Shandong Yousuo Chemical Technology Co., Ltd. / KH550; ammonium polyphosphate was purchased from: Qiansheng Chemical / 68333-79-9; polyvinyl chloride resin powder was purchased from: Taiwan Formosa Plastics / S-65 (powder); white mud was purchased from: Guangxi Huajian / specification 325 mesh; calcium phytate was purchased from Kmik.
[0018] Example 1
[0019] A flame-retardant polyvinyl chloride cable, the structure of the flame-retardant polyvinyl chloride cable from inside to outside is a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, the flame-retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.1-0.3:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:1.
[0020] The preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add modified phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
[0021] In the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 80° C. and 2 h, respectively, and the drying temperature and time are 100° C. and 24 h, respectively.
[0022] In the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g:0.1 g:800 mL, the temperature and time of the heating and stirring are 80° C. and 2 h, respectively, and the temperature and time of the drying are 100° C. and 24 h, respectively.
[0023] In the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:9g:800mL, the temperature and time of heating and stirring are 80°C and 2h respectively, and the temperature and time of drying are 100°C and 24h respectively.
[0024] The preparation method of the modified phytate in step (3) is: mixing a silane coupling agent, phytate and ammonium polyphosphate in a mass ratio of 1:0.5:30, then heating and stirring, and cooling to obtain the modified phytate, wherein the phytate is calcium phytate, and the temperature and time of heating and stirring are 100° C. and 1 h, respectively.
[0025] The preparation method of the modified white mud is as follows: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and a silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
[0026] The temperature and time of the drying and grinding are 100° C. and 24 h respectively, the particle size of the white mud powder is 3 μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50 g:500 mL:3 g, and the temperature and time of the heating and stirring are 80° C. and 5 h respectively.
[0027] The preparation process of the flame-retardant polyvinyl chloride cable is as follows: a wire core and a flame-retardant filling layer are placed in a mold, and then formed and extruded with a polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 200° C., and the wire core is an aluminum wire.
[0028] Example 2
[0029] A flame-retardant polyvinyl chloride cable, wherein the structure of the flame-retardant polyvinyl chloride cable from inside to outside is a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, wherein the flame-retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.2:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:1.
[0030] The preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add modified phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
[0031] In the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 90° C. and 2.5 h, respectively, and the drying temperature and time are 105° C. and 24 h, respectively.
[0032] In the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g:0.15 g:900 mL, the temperature and time of the heating and stirring are 80° C. and 2.5 h respectively, and the temperature and time of the drying are 105° C. and 24 h respectively.
[0033] In the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:9.5g:900mL, the temperature and time of heating and stirring are 80°C and 2.5h respectively, and the temperature and time of drying are 105°C and 24h respectively.
[0034] The preparation method of the modified phytate in step (3) is: mixing a silane coupling agent, phytate and ammonium polyphosphate in a mass ratio of 1:3:35, then heating and stirring, and cooling to obtain the modified phytate, wherein the phytate is calcium phytate, and the temperature and time of heating and stirring are 125° C. and 1.5 h, respectively.
[0035] The preparation method of the modified white mud is as follows: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and a silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
[0036] The temperature and time of the drying and grinding are 105° C. and 24 h respectively, the particle size of the white mud powder is 4 μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50 g:600 mL:3 g, and the temperature and time of the heating and stirring are 80° C. and 5.5 h respectively.
[0037] The preparation process of the flame-retardant polyvinyl chloride cable is as follows: a wire core and a flame-retardant filling layer are placed in a mold, and then formed and extruded with a polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 210° C., and the wire core is an aluminum wire.
[0038] Example 3
[0039] A flame-retardant polyvinyl chloride cable, wherein the structure of the flame-retardant polyvinyl chloride cable from inside to outside is a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, wherein the flame-retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.3:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:1.
[0040] The preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add modified phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
[0041] In the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 100° C. and 3 h, respectively, and the drying temperature and time are 110° C. and 24 h, respectively.
[0042] In the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g:0.2 g:1000 mL, the heating and stirring temperature and time are 80° C. and 3 h respectively, and the drying temperature and time are 110° C. and 24 h respectively.
[0043] In the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:10g:1000mL, the temperature and time of heating and stirring are 80°C and 3h respectively, and the temperature and time of drying are 110°C and 24h respectively.
[0044] The preparation method of the modified phytate in step (3) is: mixing a silane coupling agent, phytate and ammonium polyphosphate in a mass ratio of 1:5:40, then heating and stirring, and cooling to obtain the modified phytate, wherein the phytate is calcium phytate, and the temperature and time of heating and stirring are 150° C. and 2 h, respectively.
[0045] The preparation method of the modified white mud is as follows: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and a silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
[0046] The temperature and time of the drying and grinding are 110° C. and 24 h respectively, the particle size of the white mud powder is 5 μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50 g:700 mL:3 g, and the temperature and time of the heating and stirring are 80° C. and 6 h respectively.
[0047] The preparation process of the flame-retardant polyvinyl chloride cable is as follows: a wire core and a flame-retardant filling layer are placed in a mold, and then formed and extruded with a polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 220° C., and the wire core is an aluminum wire.
[0048] Comparative Example 1 On the basis of Example 2, a flame retardant polyvinyl chloride cable is provided, wherein the structure of the flame retardant polyvinyl chloride cable from the inside to the outside is a wire core, a flame retardant filling layer and a polyvinyl chloride composite sheath, wherein the flame retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.2:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:1.
[0049] The preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
[0050] In the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 90° C. and 2.5 h, respectively, and the drying temperature and time are 105° C. and 24 h, respectively.
[0051] In the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g:0.15 g:900 mL, the temperature and time of the heating and stirring are 80° C. and 2.5 h respectively, and the temperature and time of the drying are 105° C. and 24 h respectively.
[0052] In the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:9.5g:900mL, the temperature and time of heating and stirring are 80°C and 2.5h respectively, and the temperature and time of drying are 105°C and 24h respectively.
[0053] In the step (3), the phytate is calcium phytate.
[0054] The preparation method of the modified white mud is as follows: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and a silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
[0055] The temperature and time of the drying and grinding are 105° C. and 24 h respectively, the particle size of the white mud powder is 4 μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50 g:600 mL:3 g, and the temperature and time of the heating and stirring are 80° C. and 5.5 h respectively.
[0056] The preparation process of the flame-retardant polyvinyl chloride cable is as follows: a wire core and a flame-retardant filling layer are placed in a mold, and then formed and extruded with a polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 210° C., and the wire core is an aluminum wire.
[0057] Comparative Example 2 On the basis of Example 2, the magnesium hydroxide in the polyvinyl chloride composite sheath was removed and replaced with modified basalt of equal mass, and other conditions were consistent with Example 2.
[0058] Comparative Example 3 On the basis of Example 2, the modified basalt in the polyvinyl chloride composite sheath was removed and an equal mass of magnesium hydroxide was used. Other conditions were consistent with those in Example 2.
[0059] Comparative Example 4 On the basis of Example 2, the modified white mud in the polyvinyl chloride composite sheath was removed and replaced with modified basalt of equal mass, and other conditions were consistent with Example 2.
[0060] Comparative Example 5 On the basis of Example 2, N,N'-piperazine di(methylphosphonic acid) in the flame retardant filling layer was removed, and other conditions were consistent with those in Example 2.
[0061] 1. Performance Testing Oxygen index determination: The cables prepared in Examples 1-3 and Comparative Examples 1-4 were tested for oxygen index using polyvinyl chloride composite sheaths as samples according to GB / T 2406.2-2009; Determination of smoke generation: The cables prepared in Examples 1-3 and Comparative Examples 2-5 are used as samples. The smoke generated during the combustion process is adsorbed on the container wall of the glass container used. Then, the smoke generated by each sample under flammable conditions is compared by visual inspection. If the smoke generation is small, the adsorbed smoke is small. On the contrary, if the smoke generation is large, the adsorbed smoke is large. The evaluation criteria for smoke generation are large, medium, and small. The relative size of the smoke generation of the sample can be judged according to the light transmittance of the glass tube wall.
[0062] The above test results are shown in Table 1.
[0063] Table 1 Test results
[0064] It can be concluded from Table 1 that the oxygen index of Examples 1-3 is greater than that of Comparative Examples 1-4, while the smoke emission is less than that of Comparative Examples 2-5. In Comparative Example 1, unmodified phytate is introduced into basalt, and its dispersion in polyvinyl chloride is uneven, thus affecting the flame retardancy; in Comparative Examples 2-4, one of the components of the polyvinyl chloride composite sheath is removed, and its lack of gas phase or condensed phase and heat absorption dimension causes the flame retardant effect to decrease; in Comparative Example 5, N,N'-piperazine di(methylphosphonic acid) is not added, and a large amount of smoke is generated because the free radicals in the gas phase cannot be suppressed.
[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A flame retardant polyvinyl chloride cable, characterized in that: The structure of the flame-retardant polyvinyl chloride cable from inside to outside is a wire core, a flame-retardant filling layer and a polyvinyl chloride composite sheath, the flame-retardant filling layer is composed of N,N'-piperazine di(methylphosphonic acid), modified basalt and modified white mud in a mass ratio of 0.1-0.3:1:1, and the polyvinyl chloride composite sheath is composed of polyvinyl chloride resin powder, magnesium hydroxide, modified basalt and modified white mud in a mass ratio of 10:2:1:
1.
2. A flame retardant polyvinyl chloride cable according to claim 1, characterized in that: The preparation method of the modified basalt comprises the following steps: (1) mixing basalt powder with sodium hydroxide solution, heating and stirring, filtering and washing the solid with distilled water, and drying to obtain pretreated basalt powder; (2) mixing the pretreated basalt powder, the silane coupling agent and deionized water, then heating and stirring, filtering, washing the solid with distilled water, and drying to obtain basalt powder a; (3) Basalt powder a. Add modified phytate and deionized water, heat and stir, filter, wash the solid with distilled water, and dry to obtain modified basalt.
3. A flame retardant polyvinyl chloride cable according to claim 2, characterized in that: In the step (1), the ratio of basalt powder to sodium hydroxide solution is 3:100 g / mL, wherein the molar concentration of the sodium hydroxide solution is 4 mol / L, the heating temperature and time are 80-100° C. and 2-3 h, respectively, and the drying temperature and time are 100-110° C. and 24 h, respectively.
4. A flame retardant polyvinyl chloride cable according to claim 2, characterized in that: In the step (2), the ratio of the pretreated basalt powder, the silane coupling agent and the deionized water is 1 g: 0.1-0.2 g: 800-1000 mL, the temperature and time of the heating and stirring are 80° C. and 2-3 h, respectively, and the temperature and time of the drying are 100-110° C. and 24 h, respectively.
5. The flame retardant polyvinyl chloride cable according to claim 2, characterized in that: In the step (3), the ratio of basalt powder a, modified phytate and deionized water is 5g:9-10g:800-1000mL, the temperature and time of heating and stirring are 80°C and 2-3h respectively, and the temperature and time of drying are 100-110°C and 24h respectively.
6. A flame retardant polyvinyl chloride cable according to claim 2, characterized in that: The preparation method of the modified phytate in step (3) is: mixing a silane coupling agent, phytate and ammonium polyphosphate in a mass ratio of 1:0.5-5:30-40, then heating and stirring, and cooling to obtain the modified phytate, wherein the phytate is calcium phytate, and the temperature and time of the heating and stirring are 100-150° C. and 1-2 h, respectively.
7. The flame retardant polyvinyl chloride cable according to claim 1, characterized in that: The preparation method of the modified white mud is as follows: the white mud is first dried and ground, sieved to obtain white mud powder, distilled water and a silane coupling agent are added, heated and stirred, and then washed with anhydrous ethanol, and dried to obtain the modified white mud.
8. The flame retardant polyvinyl chloride cable according to claim 7, characterized in that: The temperature and time of the drying and grinding are 100-110° C. and 24 h respectively, the particle size of the white mud powder is 3-5 μm, the ratio of the white mud powder, distilled water and silane coupling agent is 50 g:500-700 mL:3 g, and the temperature and time of the heating and stirring are 80° C. and 5-6 h respectively.
9. The flame-retardant polyvinyl chloride cable according to claim 1, characterized in that: The preparation process of the flame-retardant polyvinyl chloride cable is as follows: a wire core and a flame-retardant filling layer are placed in a mold, and then formed and extruded with a polyvinyl chloride composite sheath in an extruder to obtain a flame-retardant polyvinyl chloride cable, wherein the extrusion temperature is 200-220° C., and the wire core is an aluminum wire.
Citation Information
Patent Citations
Polyvinyl chloride insulation cable with inflaming retarding and heat resistant performance and manufacturing method thereof
CN104733116A
Organic silicon modified phytate coupled ammonium polyphosphate and fireproof coating prepared from same
CN112662012A
B1 flame-retardant cable sheath material and preparation method thereof
CN113462063A
Flame-retardant polyethylene material as well as preparation method and application thereof
CN114044954A
Outer sheath, manufacturing process thereof and B1-level low-voltage cross-linked cable with outer sheath
CN116675934A