Preparation method of sintered neodymium-iron-boron permanent magnet with complex shape

By mixing NdFeB permanent magnet powder with adhesive and additives, molding or injection molding, degumming and pressurizing sintering, combined with two sections of heat treatment, it is difficult to prepare high-performance miniaturized, complex shape NdFeB, which is difficult to prepare high-performance, compact, and shape NdFeB, through traditional methods. The problem of permanent magnets has achieved the improvement of high magnetic performance and mechanical performance, meeting the market's demand for complex-shaped products.

CN119049864APending Publication Date: 2024-11-29SICHUAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411287523.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The traditional NdFeB permanent magnet preparation method is difficult to meet the magnetic performance and mechanical performance requirements of miniaturized and complex shape products. The magnetic performance of bonded magnets is low, and it is difficult to achieve complex shape preparation for sintered magnets.

Method used

Neodymium iron boron permanent magnet powder is mixed with adhesive and additives and molded or injected to form, degumming and pressurized sintering, combined with two stages of heat treatment, and high-performance complex shape sintered neodymium iron boron permanent magnets are prepared.

Benefits of technology

It improves the magnetic and mechanical properties of neodymium iron boron permanent magnets, meets the market's demand for high-performance miniaturized and shaped complex shape products, and improves thermal stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of sintered neodymium-iron-boron permanent magnet preparation, and provides a preparation method of a sintered neodymium-iron-boron permanent magnet in a complex shape, which comprises the following steps: (1) preparing neodymium-iron-boron permanent magnet master batch for bonding; (2) carrying out compression molding or injection molding on the master batch under the condition of applying an oriented magnetic field; (3) the obtained green body is subjected to degumming treatment at 500-700 DEG C under the condition of continuous vacuumizing, vacuumizing is stopped, the temperature is increased to 900-1100 DEG C, then low-pressure sintering is conducted under the pressure of 2-5 MPa, and the green body is cooled to the room temperature along with a furnace; and (4) carrying out two-stage heat treatment. The problems that an existing neodymium-iron-boron permanent magnet is not high in magnetic performance, insufficient in mechanical strength and the like are solved, the problem that an existing sintered magnet preparation method cannot meet the design requirements of neodymium-iron-boron permanent magnet products in complex shapes such as miniaturization and special shapes is solved, and preparation of the high-magnetic-performance sintered neodymium-iron-boron permanent magnet in the complex shape is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing sintered NdFeB permanent magnets, and relates to a method for preparing a sintered NdFeB permanent magnet with a complex shape. Background Art

[0002] With the continuous development of technology, there are more and more miniaturized, complex and special-shaped product designs in the field of NdFeB permanent magnets, and at the same time, the requirements for the magnetic properties of products are getting higher and higher. In order to meet the requirements for miniaturized, complex and special-shaped products, traditional preparation technologies often use injection molding or compression molding to make bonded magnets. However, since bonded magnets contain a large amount of non-magnetic components such as adhesives, plasticizers and stabilizers, the proportion of magnetic powder filling is not high, resulting in low magnetic properties of bonded magnets. For bonded NdFeB permanent magnets, the BNM-12L bonded NdFeB permanent magnet has better magnetic properties on the market. Its magnetic properties related data: remanence Br is 750~800mT, coercive force HCB is 432~496KA / m, intrinsic coercive force HCJ is 520~640KA / m, and maximum magnetic energy product BH (max) 84~92KJ / m 3 Its magnetic properties are difficult to meet the market demand for high-performance products, and bonded magnets also have problems such as insufficient mechanical strength, poor thermal stability and poor oxidation resistance. The traditional method of preparing sintered NdFeB permanent magnets by dry pressing and orientation molding followed by high-temperature sintering can produce sintered magnets with higher magnetic properties, but it is difficult to achieve the preparation of small, complex and special-shaped NdFeB permanent magnet devices.

[0003] Although the traditional preparation method of bonded NdFeB permanent magnets can hardly meet higher magnetic performance requirements while meeting the shape and structure of magnetic devices, the traditional preparation method of sintered NdFeB permanent magnets can meet higher magnetic performance requirements, but it is difficult to meet the design and use requirements of complex shaped products such as miniaturization and special-shaped products. Therefore, it is necessary to innovate on the basis of the preparation methods of traditional bonded magnets and sintered magnets to better meet the market demand for high-performance, miniaturized, special-shaped and other complex shaped NdFeB permanent magnet components. Summary of the invention

[0004] In view of the problems that NdFeB permanent magnets prepared by the existing bonding magnet preparation method have low magnetic properties and insufficient mechanical strength, and the problem that the existing sintered magnet preparation method cannot meet the design requirements of complex-shaped NdFeB permanent magnet products such as miniaturization and special-shaped, the present invention provides a method for preparing complex-shaped sintered NdFeB permanent magnets, so as to achieve the preparation of complex-shaped sintered NdFeB permanent magnets with higher magnetic properties.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a complex-shaped sintered NdFeB permanent magnet comprises the following steps:

[0007] (1) fully mixing NdFeB permanent magnet powder with a binder and an additive to obtain a mixture, then kneading the mixture evenly and granulating it to obtain a NdFeB permanent magnet masterbatch for bonding;

[0008] (2) compression molding or injection molding the bonding NdFeB permanent magnet masterbatch, applying an oriented magnetic field during molding, and preparing a NdFeB permanent magnet green body with a desired complex shape;

[0009] (3) placing the complex-shaped NdFeB permanent magnet green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace to a pressure of 0.01 to 10Pa, then heating it to 500 to 700°C, and keeping it warm for 2 to 4 hours to perform debonding treatment. During the heating and keeping warm process, evacuating the furnace continuously to keep the pressure in the furnace at 0.01 to 10Pa. After the debonding treatment is completed, stopping evacuating the furnace, heating it to 900 to 1100°C, and then filling the low-pressure sintering furnace with nitrogen or argon to a pressure of 2 to 5MPa. Keeping it warm for 0.5 to 1 hour to perform low-pressure sintering. After the sintering is completed, cooling it to room temperature with the furnace to obtain a debonded NdFeB permanent magnet;

[0010] (4) continuing to perform two-stage heat treatment on the debonded NdFeB permanent magnet in a low-pressure sintering furnace to obtain a sintered NdFeB permanent magnet with a complex shape.

[0011] In step (1) of the technical solution of the above-mentioned preparation method, in the mixture obtained by fully mixing the NdFeB permanent magnet powder with the adhesive and the additive, the contents of the NdFeB permanent magnet powder, the adhesive and the additive are preferably 87wt% to 93wt%, 3wt% to 6wt% and 4wt% to 7wt%, respectively.

[0012] In the technical solution of the above preparation method, the adhesive includes at least one of phenolic resin, BM-2C resin, nylon 6 and paraffin.

[0013] In the technical solution of the above preparation method, the auxiliary agent includes an antioxidant and a lubricant. Further, the antioxidant is a special antioxidant for NdFeB, and the lubricant is selected from at least one of stearyl glycerol and zinc stearate and at least one of anhydrous ethanol and acetone.

[0014] In step (4) of the technical solution of the above preparation method, the operation of the two-stage heat treatment is as follows: exhausting the nitrogen or argon in the low-pressure sintering furnace after the treatment in step (3) and evacuating the furnace until the pressure in the furnace does not exceed 1×10 -2Pa, the temperature was raised to 900-920℃ and kept for 2-3h, then cooled to room temperature with the furnace, and then raised to 520-560℃ and kept for 2-3h, then cooled to room temperature with the furnace after the end of the heat preservation, to obtain a complex sintered NdFeB permanent magnet; during the heating and heat preservation process, the vacuum was continuously drawn to keep the pressure in the furnace no more than 1×10 -2 Pa.

[0015] In the technical scheme of the above preparation method, when compression molding is used in step (2) to prepare the required complex-shaped NdFeB permanent magnet green body, it is preferred to control the molding orientation magnetic field strength to at least 1.5T, the molding temperature to 120-150°C, and the molding pressure to 600-1000MPa.

[0016] In the technical scheme of the above preparation method, when injection molding is used in step (2) to prepare the required complex-shaped NdFeB permanent magnet green body, it is preferred to control the molding orientation magnetic field strength to be at least 1T, the injection temperature to be 270-300°C, the injection pressure to be 150-170MPa, and the extrusion temperature to be 230-260°C.

[0017] In step (2) of the technical solution of the above preparation method, the heating rate during heating is preferably controlled to be 2 to 5°C / min.

[0018] In step (1) of the technical solution of the above preparation method, the average particle size of the NdFeB permanent magnet powder is preferably 2 to 5 μm.

[0019] The main technical concept of the present invention is that, first, NdFeB permanent magnet powder is prepared into a bonding NdFeB permanent magnet masterbatch with a binder and an auxiliary agent, and then compression molding or injection molding is performed into a NdFeB permanent magnet green body of a desired complex shape, and then a degumming treatment is performed under a continuous vacuum condition, and the auxiliary agents of organic components such as the binder, antioxidant and lubricant are carbonized and removed, and after the degumming treatment is completed, sintering is performed under a pressurized condition (the pressure in the furnace is 2-5MPa) to increase the compactness of the magnet, and finally a complex-shaped sintered NdFeB permanent magnet is obtained through two-stage heat treatment. On the one hand, the present invention prepares the NdFeB permanent magnet green body of a desired complex shape by compression molding or injection molding from the bonding NdFeB permanent magnet masterbatch, which solves the problem that the existing preparation method of sintered NdFeB permanent magnet can meet the requirements of high magnetic properties, but is difficult to meet the design and use requirements of complex-shaped products such as miniaturization and special-shaped. On the other hand, the present invention subjects NdFeB permanent magnet green bodies of complex shapes to carbonization debinding and pressure sintering, thereby removing organic binders and additives, increasing the proportion of magnetic components and the density of the magnet, thereby improving the magnetic properties and mechanical properties of the NdFeB magnet, solving the problem that the existing preparation method of bonded NdFeB permanent magnets can meet the design and use requirements of complex-shaped products but has low magnetic properties and mechanical properties, and can also solve the problem of poor thermal stability of the magnet when used under high temperature conditions due to the presence of organic binders and additives.

[0020] Compared with the prior art, the technical solution provided by the present invention produces the following beneficial technical effects:

[0021] The present invention provides a method for preparing a sintered NdFeB permanent magnet with a complex shape. The method first forms a NdFeB permanent magnet masterbatch for bonding into a NdFeB permanent magnet green body with a desired complex shape based on compression molding or injection molding, then debonds under continuous vacuum conditions, sinters under pressure conditions, and finally prepares a sintered NdFeB permanent magnet with a complex shape through two stages of heat treatment. Compared with the prior art method of preparing a sintered NdFeB permanent magnet by first dry pressing orientation molding and then high-temperature sintering, the present invention forms a NdFeB permanent magnet masterbatch for bonding by compression molding or injection molding, realizes free molding of the NdFeB permanent magnet green body, can prepare a green body with a complex shape, and solves the problem that it is difficult to prepare small, complex, and special-shaped NdFeB permanent magnet devices in the existing method for preparing sintered NdFeB permanent magnets. Compared with the existing method for preparing bonded NdFeB permanent magnets, which is to mix a large amount of adhesives, plasticizers and stabilizers with magnetic powders and then form them freely, the present invention carbonizes the green body of complex shape under continuous vacuum conditions at high temperature, so that the adhesive and auxiliary agents of organic components are pyrolyzed and removed, and then sintered under pressure, which increases the proportion of magnetic components and the density of the magnet, thereby improving the magnetic properties and mechanical properties of the NdFeB magnet, and solves the problems of low magnetic properties and mechanical properties of existing bonded NdFeB permanent magnets, as well as poor thermal stability when used under high temperature conditions. The method of the present invention can realize the preparation of sintered NdFeB permanent magnets with complex shapes and high magnetic properties, and can better meet the market demand for high-performance, miniaturized, and special-shaped NdFeB permanent magnet components with complex shapes. DETAILED DESCRIPTION

[0022] The following examples further illustrate the preparation method of the complex-shaped sintered NdFeB permanent magnet provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The technical personnel in the relevant field make some non-essential improvements and adjustments to the present invention according to the above invention content for specific implementation, which still falls within the scope of protection of the present invention.

[0023] Example 1

[0024] In this embodiment, a method for preparing a sintered NdFeB permanent magnet with a complex shape is provided, and the steps are as follows:

[0025] (1) The NdFeB permanent magnet powder is passed through a 60-80 mesh sieve to obtain NdFeB permanent magnet powder with an average particle size of 3.0 μm.

[0026] (2) NdFeB permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the ingredients are prepared according to the ratio of 87.13wt%, 5.94wt% and 6.93wt% of the contents of NdFeB permanent magnet powder, adhesive and auxiliary agent in all raw materials. The adhesive is phenolic resin and BM-2C resin, and the auxiliary agent includes lubricant and antioxidant. The antioxidant is a commercially available NdFeB special antioxidant, and the lubricant is glyceryl stearate and anhydrous ethanol.

[0027] Weigh 880g of NdFeB permanent magnet powder with an average particle size of 3.0μm, 30g of phenolic resin, 30g of BM-2C resin, 5g of commercially available NdFeB special antioxidant, 5g of stearic acid glyceryl ester, and 60g of anhydrous ethanol. Stir and mix the weighed raw materials thoroughly, heat and mix the resulting mixture on a double-roll mixer, and then granulate it to make a NdFeB permanent magnet masterbatch for bonding.

[0028] (3) The bonding NdFeB permanent magnet masterbatch is compression molded on a compression molding device, and an orientation magnetic field is applied during the molding process to prepare the NdFeB permanent magnet green body with the required complex shape. The molding orientation magnetic field strength is controlled to be 1.5T, the molding temperature is 120°C, and the molding pressure is 600MPa.

[0029] (4) placing the green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace until the pressure inside the furnace is 10Pa, then heating the temperature to 550°C at a heating rate of 3°C / min, and keeping the temperature for 4 hours to perform debinding and decarburization treatment. During the heating and keeping temperature process, continuously evacuating the temperature to maintain the pressure inside the furnace at a level of 0.01 to 10Pa. After the debinding and decarburization treatment is completed, stopping evacuating the temperature, heating the temperature to 1100°C at a heating rate of 3°C / min, filling the low-pressure sintering furnace with argon until the pressure inside the furnace is 5MPa, and keeping the temperature for 1 hour to perform low-pressure sintering. After the sintering is completed, cooling the furnace to room temperature to obtain a debonded NdFeB permanent magnet.

[0030] (5) Exhaust the argon gas in the low-pressure sintering furnace after the treatment in step (4) and evacuate the furnace until the pressure in the furnace does not exceed 1×10 -2 Pa, and then the temperature was raised to 900℃ and kept for 2 hours. After the heat preservation, the furnace was cooled to room temperature, and then the temperature was raised to 530℃ and kept for 2 hours. After the heat preservation, the furnace was cooled to room temperature to obtain a complex-shaped sintered NdFeB permanent magnet. During the heating and heat preservation process, the vacuum was continuously drawn to keep the pressure in the furnace no more than 1×10 -2 Pa.

[0031] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence Br was 1180mT, the coercive force HCB was 650KA / m, the intrinsic coercive force HCJ was 755KA / m, and the maximum magnetic energy product BH (max) 282KJ / m 3 .

[0032] Example 2

[0033] In this embodiment, a method for preparing a sintered NdFeB permanent magnet with a complex shape is provided, and the steps are as follows:

[0034] (1) The NdFeB permanent magnet powder is passed through a 60-80 mesh sieve to obtain NdFeB permanent magnet powder with an average particle size of 3.0 μm.

[0035] (2) NdFeB permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the ingredients are prepared according to the ratio of 90wt%, 5wt% and 5wt% of the content of NdFeB permanent magnet powder, adhesive and auxiliary agent in all raw materials. The adhesive is paraffin and BM-2C resin, and the auxiliary agent includes an antioxidant and a lubricant. The antioxidant is a commercially available antioxidant special for NdFeB, and the lubricant is zinc stearate and anhydrous ethanol.

[0036] Weigh 900g of NdFeB permanent magnet powder with an average particle size of 3.0μm, 20g of paraffin wax, 30g of BM-2C resin, 3g of commercially available NdFeB special antioxidant, 5g of zinc stearate, and 42g of anhydrous ethanol. Stir and mix the weighed raw materials thoroughly, heat and mix the resulting mixture on a double-roll mixer, and then granulate it to make a NdFeB permanent magnet masterbatch for bonding.

[0037] (3) The bonding NdFeB permanent magnet masterbatch is molded by an injection molding device, and an orientation magnetic field is applied during the molding to prepare the NdFeB permanent magnet green body with the required complex shape. The molding orientation magnetic field strength is controlled to be 1T, the injection temperature is 285°C, the injection pressure is 160MPa, and the extrusion temperature is 245°C.

[0038] (4) placing the green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace until the pressure inside the furnace is 0.1 Pa, then heating the temperature to 650°C at a heating rate of 4°C / min, and keeping the temperature for 3 hours to perform debinding and decarburization treatment. During the heating and insulation process, vacuuming is continuously performed to maintain the pressure inside the furnace at a level of 0.01 to 0.1 Pa. After the debinding and decarburization treatment is completed, vacuuming is stopped, heating the temperature to 1000°C at a heating rate of 3°C / min, argon is filled into the low-pressure sintering furnace until the pressure inside the furnace is 4MPa, and the temperature is kept for 0.75 hours to perform low-pressure sintering. After the sintering is completed, the furnace is cooled to room temperature to obtain a debonded NdFeB permanent magnet.

[0039] (5) Exhaust the argon gas in the low-pressure sintering furnace after the treatment in step (4) and evacuate the furnace until the pressure in the furnace does not exceed 1×10 -2 Pa, and then the temperature was raised to 910℃ and kept for 2h. After the heat preservation, the furnace was cooled to room temperature. Then the temperature was raised to 540℃ and kept for 2h. After the heat preservation, the furnace was cooled to room temperature. Complex sintered NdFeB permanent magnets were obtained. During the heating and heat preservation process, the vacuum was continuously drawn to keep the pressure in the furnace no more than 1×10 -2Pa.

[0040] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence Br was 1280mT, the coercive force HCB was 720KA / m, the intrinsic coercive force HCJ was 810KA / m, and the maximum magnetic energy product BH (max) 298KJ / m 3 .

[0041] Example 3

[0042] In this embodiment, a method for preparing a sintered NdFeB permanent magnet with a complex shape is provided, and the steps are as follows:

[0043] (1) The NdFeB permanent magnet powder is passed through a 60-80 mesh sieve to obtain NdFeB permanent magnet powder with an average particle size of 3.0 μm.

[0044] (2) NdFeB permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the content of NdFeB permanent magnet powder, adhesive and auxiliary agent in all raw materials is 93wt%, 3wt% and 4wt% respectively. The adhesive is nylon 6 (PA6) and BM-2C resin. The auxiliary agent includes an antioxidant and a lubricant. The antioxidant is a commercially available antioxidant special for NdFeB. The lubricant is zinc stearate and anhydrous ethanol.

[0045] Weigh 900g of NdFeB permanent magnet powder with an average particle size of 3.0μm, 15g of nylon 6 (PA6), 15g of BM-2C resin, 3g of commercially available NdFeB special antioxidant, 2g of zinc stearate, and 35g of anhydrous ethanol. Stir and mix the weighed raw materials thoroughly, heat and mix the resulting mixture evenly on a double-roll mixer, and then granulate it to make a NdFeB permanent magnet masterbatch for bonding.

[0046] (3) The bonding NdFeB permanent magnet masterbatch is compression molded on a compression molding device, and an orientation magnetic field is applied during the molding process to prepare the NdFeB permanent magnet green body with the required complex shape. The molding orientation magnetic field strength is controlled to be 2.0T, the molding temperature is 120°C, and the molding pressure is 900MPa.

[0047] (4) Place the complex-shaped NdFeB permanent magnet green body in a low-pressure sintering furnace, evacuate the low-pressure sintering furnace until the pressure in the furnace is 0.01Pa, then heat it to 650℃ at a heating rate of 4℃ / min, and keep it at that temperature for 3h for debinding and decarburization treatment. During the heating and keeping process, continue to evacuate the furnace to keep the pressure in the furnace at 0.01Pa. After the debinding and decarburization treatment is completed, stop evacuating the furnace, heat it to 910℃ at a heating rate of 5℃ / min, fill the low-pressure sintering furnace with argon until the pressure in the furnace is 3MPa, keep it at that temperature for 0.5h for low-pressure sintering. After the sintering is completed, cool it to room temperature with the furnace to obtain a debonded NdFeB permanent magnet.

[0048] (5) Exhaust the argon gas in the low-pressure sintering furnace after the treatment in step (4) and evacuate the furnace until the pressure in the furnace does not exceed 1×10 -2 Pa, and then the temperature was raised to 915℃ and kept for 2 hours. After the heat preservation, the furnace was cooled to room temperature, and then the temperature was raised to 550℃ and kept for 2 hours. After the heat preservation, the furnace was cooled to room temperature to obtain a complex-shaped sintered NdFeB permanent magnet. During the heating and heat preservation process, the vacuum was continuously drawn to keep the pressure in the furnace no more than 1×10 -2 Pa.

[0049] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence Br was 1350mT, the coercive force HCB was 750KA / m, the intrinsic coercive force HCJ was 825KA / m, and the maximum magnetic energy product BH (max) 315KJ / m 3 .

[0050] At present, the bonded NdFeB permanent magnet with better magnetic properties on the market is BNM-12L bonded NdFeB permanent magnet. Its magnetic properties are as follows: remanence Br is 750-800mT, coercive force HCB is 432-496KA / m, intrinsic coercive force HCJ is 520-640KA / m, maximum magnetic energy product BH (max) 84~92KJ / m 3 . In combination with Examples 1 to 3, it can be seen that the magnetic properties of the complex-shaped sintered NdFeB permanent magnets prepared by the method of the present invention are significantly better than those of the BNM-12L bonded NdFeB permanent magnets. At the same time, since the method of the present invention performs debonding and pressure sintering, the density of the magnet is further increased on the basis of removing the adhesive and additives of the organic components. Therefore, compared with the existing bonded NdFeB permanent magnets, the complex-shaped sintered NdFeB permanent magnets prepared by the method of the present invention are also more advantageous in terms of mechanical properties, and can better meet the market demand for high-performance, miniaturized, and special-shaped NdFeB permanent magnet components with complex shapes.

Claims

1. A method for preparing complex-shaped sintered NdFeB permanent magnets. It is characterized in that The following steps are involved: (1) fully mixing NdFeB permanent magnet powder with a binder and an additive to obtain a mixture, then kneading the mixture evenly and granulating it to obtain a NdFeB permanent magnet masterbatch for bonding; (2) compression molding or injection molding the bonding NdFeB permanent magnet masterbatch, applying an oriented magnetic field during molding, and preparing a NdFeB permanent magnet green body with a desired complex shape; (3) placing the complex-shaped NdFeB permanent magnet green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace to a pressure of 0.01 to 10Pa, then heating it to 500 to 700°C, and keeping it warm for 2 to 4 hours to perform debonding treatment. During the heating and keeping warm process, evacuating the furnace continuously to keep the pressure in the furnace at 0.01 to 10Pa. After the debonding treatment is completed, stopping evacuating the furnace, heating it to 900 to 1100°C, and then filling the low-pressure sintering furnace with nitrogen or argon to a pressure of 2 to 5MPa. Keeping it warm for 0.5 to 1 hour to perform low-pressure sintering. After the sintering is completed, cooling it to room temperature with the furnace to obtain a debonded NdFeB permanent magnet; (4) continuing to perform two-stage heat treatment on the debonded NdFeB permanent magnet in a low-pressure sintering furnace to obtain a sintered NdFeB permanent magnet with a complex shape.

2. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to claim 1, It is characterized in that In step (1), the NdFeB permanent magnet powder is fully mixed with a binder and an additive to obtain a mixture, wherein the contents of the NdFeB permanent magnet powder, the binder and the additive are 87wt% to 93wt%, 3wt% to 6wt% and 4wt% to 7wt% respectively.

3. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to claim 1, It is characterized in that The adhesive includes at least one of phenolic resin, BM-2C resin, nylon 6 and paraffin.

4. The method for preparing a complex-shaped sintered NdFeB permanent magnet according to claim 1, It is characterized in that The auxiliary agents include antioxidants and lubricants.

5. The method for preparing a complex-shaped sintered NdFeB permanent magnet according to claim 4, It is characterized in that The antioxidant is a special antioxidant for NdFeB, and the lubricant is selected from at least one of stearyl glycerol and zinc stearate and any one of anhydrous ethanol and acetone.

6. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to any one of claims 1 to 5, It is characterized in that The operation of the two-stage heat treatment in step (4) is as follows: exhaust the nitrogen or argon in the low-pressure sintering furnace after the treatment in step (3) and evacuate the furnace until the pressure in the furnace does not exceed 1×10 -2 Pa, the temperature was raised to 900-920℃ and kept for 2-3h, then cooled to room temperature with the furnace, and then raised to 520-560℃ and kept for 2-3h, then cooled to room temperature with the furnace after the end of the heat preservation, to obtain a complex sintered NdFeB permanent magnet; during the heating and heat preservation process, the vacuum was continuously drawn to keep the pressure in the furnace no more than 1×10 -2 Pa.

7. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to any one of claims 1 to 5, It is characterized in that When compression molding is used in step (2) to prepare the required complex-shaped NdFeB permanent magnet green body, the molding orientation magnetic field strength is controlled to be at least 1.5T, the molding temperature is 120-150°C, and the molding pressure is 600-1000MPa.

8. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to any one of claims 1 to 5, It is characterized in that When injection molding is used in step (2) to prepare the required complex-shaped NdFeB permanent magnet green body, the molding orientation magnetic field strength is controlled to be at least 1T, the injection temperature is 270-300°C, the injection pressure is 150-170MPa, and the extrusion temperature is 230-260°C.

9. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to any one of claims 1 to 5, It is characterized in that The heating rate during the temperature increase in step (3) is controlled to be 2 to 5°C / min.

10. The method for preparing the complex-shaped sintered NdFeB permanent magnet according to any one of claims 1 to 5, It is characterized in that The average particle size of the NdFeB permanent magnet powder in step (1) is 2 to 5 μm.

Citation Information

Cited By

  • MIM neodymium iron boron screening internal mixer

    CN120839060A

  • Composite metal powder injection molding neodymium-iron-boron magnet and preparation method thereof

    CN122393094A