Method for prolonging service life of quartz piece
By forming an oxygen-containing silicon carbide film layer on the surface of the quartz parts, the problem of fragility of quartz parts in the LPCVD process is solved, and its service life is extended to more than 2 years, achieving better durability and high-temperature and low-temperature alternating ability.
Patent Information
- Application Number
- CN202411076491.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the LPCVD process, the quartz parts are easy to shatter and have a short service life. The existing protective layer method is not effective, so it cannot effectively extend the service life of the quartz parts.
An oxygen-containing silicon carbide film layer is formed on the surface of the quartz piece, and a silicon carbide film is deposited on the surface of the quartz piece by chemical vapor deposition method to adjust the pressure and oxygen elements are introduced to form an oxygen-containing silicon carbide film layer of 0.2~1.5mm thick to avoid Silicon adhesion and internal stress generation.
It significantly extends the service life of quartz parts to more than 2 years, avoids surface fragmentation problems, and improves the durability and high-temperature and low-temperature alternating ability of quartz parts.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic solar energy, and in particular to a method for extending the service life of a quartz piece. Background Art
[0002] With the continuous use of human energy, non-renewable energy is becoming increasingly exhausted, and the photovoltaic solar cell industry has begun to rise. Solar power generation has gradually replaced thermal power generation. After years of research and development of solar cells, N-type Topcon batteries have been promoted and mass-produced as an emerging development direction.
[0003] Low-pressure chemical vapor deposition (LPCVD) technology is widely used in the manufacture of photovoltaic cells, especially in the manufacture of N-type Topcon cells. The thin films grown by LPCVD have good uniformity and density, and low gas consumption. Therefore, it is widely used in the production process of Topcon cells such as silicon oxide (SiO2), low-stress silicon nitride (Si3H4), and polycrystalline silicon (Poly).
[0004] The chamber and carrier components of LPCVD are mainly quartz parts, which are made of quartz and mainly composed of silicon dioxide. The reaction temperature is high when using LPCVD technology to deposit silicon oxide, low-stress silicon nitride, etc., which is often accompanied by the formation of silicon, which adheres to the quartz parts and forms hard contact with silicon dioxide. After multiple high and low temperature alternating environments, the quartz parts are stretched by stress, causing the quartz parts to break. Therefore, the problem of short service life of quartz parts in the current LPCVD process is particularly prominent. For manufacturers of N-type Topcon batteries, in today's mass production competition, cost control of the LPCVD process in its manufacturing process and improvement of the short service life of quartz parts have a very large impact on the control of battery manufacturing costs.
[0005] Regarding the service life of quartz parts, currently, the mainstream solution is to form a protective layer on their surface. If other materials are directly replaced as the main materials for LPCVD chambers and carriers, the cost will be greatly increased, which will not play a role in controlling costs. Quartz materials are cheap and easy to obtain, so it is still cheaper to keep quartz as the main material. However, the current method of forming a protective layer on the surface of quartz parts to extend the service life of quartz parts is not effective.
[0006] For example, the patent application publication number CN115448612A discloses a quartz protection treatment method, which grows a layer of aluminum oxide film on the surface of the quartz part to protect the quartz part, thereby extending the service life of the quartz part and reducing the production cost of the battery. However, the method provided by the patent only uses a thin film to isolate the silicon generated in the battery LPCVD process directly on the quartz part body, and cannot significantly extend the service life of the quartz part. After a period of use, a thick layer of reactants will still be deposited on the surface of the aluminum oxide film layer of the quartz part, resulting in the surface of the quartz part being broken. Therefore, the service life of the quartz part is still not effectively improved. Summary of the invention
[0007] In view of the problem that quartz parts in LPCVD chambers are easy to break, the present invention provides a method for extending the service life of quartz parts. The present invention forms an oxygen-containing silicon carbide film layer on the surface of the quartz parts to avoid the generation of silicon on the surface of the quartz parts, thereby greatly improving the internal stress of the quartz parts after long-term use, and in particular, greatly improving the stress of the surface layer of the quartz parts, so that the quartz parts do not have the problem of surface breakage after long-term use, and the service life of the quartz parts can be extended to more than 2 years.
[0008] The specific technical scheme of the present invention is: The present invention provides a method for extending the service life of a quartz piece, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber; Step S2: adjusting the pressure of the chamber to subnormal pressure, introducing a silicon source and a carbon source into the chamber, so as to deposit a silicon carbide film layer on the surface of the quartz piece; Step S3: adjusting the pressure of the chamber to 0.1-50 torr, and continuously introducing a silicon source and a carbon source into the chamber, and introducing an oxygen source into the chamber, so as to inject oxygen into the silicon carbide film layer on the surface of the quartz piece; wherein the introduction flow ratio of the silicon source to the oxygen source is 1:2-4; Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0009] Currently, the quartz parts in the LPCVD chamber are prone to breakage. During the LPCVD process of Topcon battery production, silicon is produced, which then adheres to the surface of the quartz parts and causes them to break.
[0010] The present invention aims at the problem of quartz parts being broken due to silicon adhering to the quartz parts. By forming an oxygen-containing silicon carbide film layer on the surface of the quartz parts, silicon is prevented from being generated on the surface of the quartz parts, and the internal stress of the quartz parts after long-term use is greatly improved. In particular, the stress of the surface layer of the quartz parts is greatly improved, so that the quartz parts do not have the problem of surface breakage after long-term use, and the service life of the quartz parts can be extended to more than 2 years.
[0011] Specifically, the quartz parts are wafer carrier quartz boats, quartz boat holders, quartz paddles, quartz tubes or furnace lining tubes used in the LPCVD process involved in the production of solar cells.
[0012] As a preferred embodiment of the above method, in step S2, the sub-atmospheric pressure is 500-700 torr.
[0013] The formation of the oxygen-containing silicon carbide film layer of the present invention first requires that in step S2, the chemical vapor deposition chamber is placed at a sub-normal pressure of 500-700 torr to deposit a preliminary silicon carbide film, and then in step S3, oxygen is injected while the silicon carbide film is deposited. When injecting oxygen, the chemical vapor deposition chamber needs to be placed at a relatively low pressure of 0.1-50 torr.
[0014] As a preferred embodiment of the above method, in step S2, the flow rate of the silicon source is 1-20 L / min, and the flow rate of the carbon source is 1-20 L / min.
[0015] As a preferred embodiment of the above method, in step S2, the time for introducing the silicon source and the carbon source is 10 to 40 minutes.
[0016] As a preferred embodiment of the above method, in step S3, the oxygen source is introduced for 5 to 20 minutes.
[0017] As a preferred embodiment of the above method, the thickness of the silicon carbide film layer is 0.2-1.5 mm.
[0018] The silicon carbide film layer deposited on the surface of the quartz piece of the present invention preferably has a thickness of 0.2 to 1.5 mm. The quartz piece is used in the LPCVD process involved in the production of solar cells. Therefore, most of its usage scenarios are high-temperature scenarios. If the thickness of the silicon carbide film is greater than 1.5 mm, the silicon carbide film layer is easy to fall off after multiple alternations of high and low temperatures; if the thickness of the silicon carbide film is less than 0.2 mm, the isolation protection effect is poor.
[0019] As a preferred embodiment of the above method, in steps S2 and S3, the temperature of the chamber is adjusted to 1200-1350°C.
[0020] As a preferred embodiment of the above method, the silicon source is monosilane and / or disilane; the carbon source is propane and / or ethylene; and the oxygen source is oxygen.
[0021] Compared with the prior art, the present invention has the following technical effects: (1) The present invention aims to solve the problem of quartz parts being broken due to silicon adhering to the quartz parts. By forming an oxygen-containing silicon carbide film layer on the surface of the quartz parts, silicon is prevented from being generated on the surface of the quartz parts, thereby greatly improving the internal stress of the quartz parts after long-term use. In particular, the stress of the surface layer of the quartz parts is greatly improved, so that the quartz parts will not have the problem of surface breakage after long-term use, and the service life of the quartz parts can be extended to 2 years.
[0022] (2) The formation of the oxygen-containing silicon carbide film layer on the surface of the quartz piece of the present invention can firstly play the role of a connecting layer between the quartz piece substrate and the attached impurities such as silicon oxide and silicon nitride generated after the process is used, thereby preventing the attached impurities generated after the process is used from directly adhering to the quartz substrate to generate large internal stress, thereby straining the quartz piece and causing cracks or fragments on the surface of the quartz piece. The present invention forms the oxygen-containing silicon carbide film layer in advance before the battery production process is used by chemical vapor deposition, which can be well integrated with the surface of the quartz substrate and the attached impurities formed after the process is used, thereby avoiding the generation of internal stress. Secondly, the production of silicon is the main reason for the damage to quartz parts. The formation of the oxygen-containing silicon carbide film layer on the surface of the quartz parts, in particular, due to the injection of a large amount of oxygen elements, can prevent the production of silicon during the process. Other attached impurities, such as silicon nitride, silicon oxide, etc., can be dissolved in the surface of the quartz part with the silicon carbide layer set on the surface of the quartz part, and the internal stress generated on the surface of the quartz part is small. Therefore, compared with the traditional isolation protective film layer, the oxygen-containing silicon carbide film layer of the present invention can play a better role in extending the service life. DETAILED DESCRIPTION
[0023] The quartz parts described in the present invention are wafer-carrying quartz boats, quartz boat holders, quartz paddles, quartz tubes or furnace lining tubes used in LPCVD processes, specifically LPCVD processes involved in solar cell production.
[0024] In order to prevent silicon from adhering to the surface of the quartz part, the traditional and mainstream practice is to form an isolation protection layer on the surface of the quartz part to prevent silicon from directly adhering to the surface of the quartz part, thereby extending its service life. For example, in the prior art, an aluminum oxide film is formed on the surface of the quartz part, and the aluminum oxide film plays an isolation and protection role on the quartz part to prevent silicon from directly adhering to the quartz part. However, these traditional isolation protection film layers cannot prevent the generation of silicon. After a period of use, some silicon will still adhere, so it is necessary to use acid or alkali to clean it. However, frequent acid and alkali cleaning will cause the quartz part to be corroded and damaged. Therefore, the traditional isolation protection film layer has a limited effect on extending the service life of the quartz part.
[0025] The present invention forms an oxygen-containing silicon carbide film layer on the surface of the quartz piece. First, it can play the role of a connecting layer between the quartz piece substrate and the attached impurities such as silicon oxide and silicon nitride generated after the process is used, so as to avoid the attached impurities generated after the process is used directly adhering to the quartz substrate to generate large internal stress, pull the quartz piece, and cause cracks or fragments on the surface of the quartz piece. Specifically, the present invention forms the oxygen-containing silicon carbide film layer in advance before the battery production process is used by chemical vapor deposition. The film layer can be well integrated with the surface of the quartz substrate and integrated with the attached impurities formed after the process is used, thereby avoiding the generation of internal stress. Secondly, the production of silicon is the main reason for the damage to quartz parts. The formation of the oxygen-containing silicon carbide film layer on the surface of the quartz parts, in particular, due to the injection of a large amount of oxygen elements, can prevent the production of silicon during the process. Other attached impurities, such as silicon nitride, silicon oxide, etc., can be dissolved in the surface of the quartz part with the silicon carbide layer set on the surface of the quartz part, and the internal stress generated on the surface of the quartz part is small. Therefore, compared with the traditional isolation protective film layer, the oxygen-containing silicon carbide film layer of the present invention can play a better role in extending the service life.
[0026] The present invention is further described below in conjunction with embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0027] Example 1 A method for extending the service life of a quartz part is provided, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber.
[0028] Step S2: The temperature of the chamber is adjusted to 1250°C and the pressure is adjusted to 600 torr, and then silicon source monosilane and carbon source propane are introduced into the chamber for 20 minutes to initially deposit a silicon carbide film on the surface of the quartz piece. The flow rate of the silicon source is 10 L / min, and the flow rate of the carbon source is 10 L / min.
[0029] Step S3: Keep introducing silicon source and carbon source into the chamber, keep the temperature constant, adjust the chamber pressure to 10torr, and introduce oxygen into the chamber at a flow rate of 40L / min, so that oxygen is injected into the silicon carbide film layer on the surface of the quartz piece. The oxygen is introduced for 10min. After step S2 and this step, an oxygen-containing silicon carbide film layer with a thickness of 1.0mm is formed on the surface of the quartz piece. In the process of injecting oxygen, the introduction flow rate ratio of silicon source to oxygen is 1:4.
[0030] Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0031] Example 2 A method for extending the service life of a quartz part is provided, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber.
[0032] Step S2: The temperature of the chamber is adjusted to 1200°C and the pressure is adjusted to 500 torr, and then silicon source monosilane and carbon source propane are introduced into the chamber for 10 minutes to initially deposit a silicon carbide film on the surface of the quartz piece. The flow rate of the silicon source is 10 L / min, and the flow rate of the carbon source is 10 L / min.
[0033] Step S3: Keep introducing silicon source and carbon source into the chamber, keep the temperature constant, adjust the pressure of the chamber to 2 torr, and introduce oxygen into the chamber at a flow rate of 20 L / min, so that oxygen is injected into the silicon carbide film layer on the surface of the quartz piece. The oxygen is introduced for 20 minutes. After step S2 and this step, an oxygen-containing silicon carbide film layer with a thickness of 0.2 mm is formed on the surface of the quartz piece. In the process of injecting oxygen, the introduction flow rate ratio of the silicon source to the oxygen is 1:2.
[0034] Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0035] Example 3 A method for extending the service life of a quartz part is provided, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber.
[0036] Step S2: The temperature of the chamber is adjusted to 1300°C and the pressure is adjusted to 700 torr, and then silicon source monosilane and carbon source propane are introduced into the chamber for 40 minutes to initially deposit a silicon carbide film on the surface of the quartz piece. The flow rate of the silicon source is 15 L / min, and the flow rate of the carbon source is 15 L / min.
[0037] Step S3: Keep introducing silicon source and carbon source into the chamber, keep the temperature constant, adjust the pressure of the chamber to 20torr, and introduce oxygen into the chamber at a flow rate of 45L / min, so that oxygen is injected into the silicon carbide film layer on the surface of the quartz piece. The oxygen is introduced for 5 minutes. After step S2 and this step, an oxygen-containing silicon carbide film layer with a thickness of 1.5mm is formed on the surface of the quartz piece. In the process of injecting oxygen, the introduction flow rate ratio of silicon source to oxygen is 1:3.
[0038] Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0039] Example 4 A method for extending the service life of a quartz part is provided, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber.
[0040] Step S2: The temperature of the chamber is adjusted to 1250°C and the pressure is adjusted to 600 torr, and then silicon source monosilane and carbon source propane are introduced into the chamber for 20 minutes to initially deposit a silicon carbide film on the surface of the quartz piece. The flow rate of the silicon source is 10 L / min, and the flow rate of the carbon source is 10 L / min.
[0041] Step S3: Keep introducing silicon source and carbon source into the chamber, keep the temperature constant, adjust the pressure of the chamber to 30torr, and introduce oxygen into the chamber at a flow rate of 40L / min, so that oxygen is injected into the silicon carbide film layer on the surface of the quartz piece. The oxygen is introduced for 10 minutes. After step S2 and this step, an oxygen-containing silicon carbide film layer with a thickness of 1.0mm is formed on the surface of the quartz piece. In the process of injecting oxygen, the introduction flow rate ratio of the silicon source to the oxygen is 1:4.
[0042] Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0043] Example 5 A method for extending the service life of a quartz part is provided, comprising the following steps: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber.
[0044] Step S2: The temperature of the chamber is adjusted to 1250°C and the pressure is adjusted to 600 torr, and then silicon source monosilane and carbon source propane are introduced into the chamber for 20 minutes to initially deposit a silicon carbide film on the surface of the quartz piece. The flow rate of the silicon source is 10 L / min, and the flow rate of the carbon source is 10 L / min.
[0045] Step S3: Keep introducing silicon source and carbon source into the chamber, keep the temperature constant, adjust the chamber pressure to 50torr, and introduce oxygen into the chamber at a flow rate of 40L / min, so that oxygen is injected into the silicon carbide film layer on the surface of the quartz piece. The oxygen is introduced for 10 minutes. After step S2 and this step, an oxygen-containing silicon carbide film layer with a thickness of 1.0mm is formed on the surface of the quartz piece. In the process of injecting oxygen, the introduction flow rate ratio of silicon source to oxygen is 1:4.
[0046] Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
[0047] Comparative Example 1 This comparative example aims to study the effect of the presence or absence of an oxygen-containing silicon carbide film layer on the service life of a quartz component.
[0048] The main difference between this comparative example and Example 1 is that: Step S2 and Step S3 are not performed to deposit the oxygen-containing silicon carbide film layer, and the quartz piece is directly put into use.
[0049] Comparative Example 2 This comparative example aims to study the influence of the oxygen-containing elements of the oxygen-containing silicon carbide film layer on the service life of the quartz parts.
[0050] The main difference between this comparative example and Example 1 is that in step S3, the silicon source and the carbon source are kept introduced into the chamber for 10 minutes, and oxygen is not introduced during this process, so that after steps S2 and S3, a silicon carbide film layer with a thickness of 1.0 mm is formed on the surface of the quartz piece. The other steps and operations are the same as those in Example 1.
[0051] Comparative Example 3 This comparative example aims to study the effect of the flow ratio of silicon source and oxygen on the oxygen content during the process of injecting oxygen element.
[0052] The main difference between this comparative example and Example 1 is that in step S3, the flow rate ratio of the silicon source to the oxygen is 1:1. The other steps and operations are the same as those in Example 1.
[0053] Comparative Example 4 This comparative example aims to study the effect of the flow ratio of silicon source and oxygen on the oxygen content during the process of injecting oxygen element.
[0054] The main difference between this comparative example and Example 1 is that in step S3, the flow rate ratio of the silicon source to the oxygen is 1:5. The other steps and operations are the same as those in Example 1.
[0055] Comparative Example 5 This comparative example aims to adjust the deposition time of the oxygen-containing silicon carbide film layer so that the thickness of the formed oxygen-containing silicon carbide film layer is different from that of Example 1, so as to study the influence of oxygen-containing silicon carbide film layers of different thicknesses on the service life of the quartz component.
[0056] The main difference between this comparative example and Example 1 is that the introduction time of the silicon source and the carbon source in step S2 is 5 minutes, and the introduction time of the silicon source, the carbon source, and the oxygen source in step S3 is 6 minutes, so that after step S2 and step S3, an oxygen-containing silicon carbide film layer with a thickness of 0.1 mm is formed on the surface of the quartz piece. The other steps and operations are the same as those in Example 1.
[0057] Comparative Example 6 This comparative example aims to adjust the deposition time of the oxygen-containing silicon carbide film layer so that the thickness of the formed oxygen-containing silicon carbide film layer is different from that of Example 1, so as to study the influence of oxygen-containing silicon carbide film layers of different thicknesses on the service life of the quartz component.
[0058] The main difference between this comparative example and Example 1 is that the introduction time of the silicon source and the carbon source in step S2 is 40 minutes, and the introduction time of the silicon source, the carbon source, and the oxygen source in step S3 is 10 minutes, so that after step S2 and step S3, an oxygen-containing silicon carbide film layer with a thickness of 1.8 mm is formed on the surface of the quartz piece. The other steps and operations are the same as those in Example 1.
[0059] Effect Characterization The service life of the quartz parts put into production in Examples 1 to 5 and Comparative Examples 1 to 6 was recorded, and the results are shown in Table 1. Among them, the quartz parts to be tested (quartz boats) were used in the LPCVD process of Topcon cells to deposit tunnel oxide layers, and the LPCVD working time, that is, the service life of the quartz parts was 12 hours / day.
[0060] Table 1 Group Service life / month Example 1 26.4 Example 2 26.0 Example 3 26.1 Example 4 24.3 Example 5 24.0 Comparative Example 1 2.2 Comparative Example 2 12.6 Comparative Example 3 14.5 Comparative Example 4 14.4 Comparative Example 5 16.9 Comparative Example 6 15.7 Data Analysis: (1) It can be seen from the service life data of Examples 1 to 5 that the present invention forms an oxygen-containing silicon carbide film layer on the surface of the quartz part to avoid the generation of silicon on the surface of the quartz part, thereby greatly improving the internal stress of the quartz part after long-term use. In particular, the stress on the surface of the quartz part is greatly improved, so that the quartz part does not have the problem of surface cracking after long-term use, and the service life of the quartz part can be extended to more than 2 years.
[0061] (2) From the comparative analysis of Examples 4-5 and Example 1, it can be seen that when injecting oxygen, the pressure in the LPCVD chamber of Example 4 and Example 5 is 30 torr and 50 torr respectively. The service life of Example 4 and Example 5 is slightly shortened compared with that of Example 1. It can be seen that when injecting oxygen, the process pressure may have a certain influence on the oxygen content of the silicon carbide film layer formed on the surface. When the chamber pressure is low, it is easy to inject oxygen into the silicon carbide film layer, and the service life of the obtained quartz parts is longer.
[0062] (3) From the comparative analysis of Comparative Examples 1-2 and Example 1, it can be seen that Comparative Example 1 does not set a thin film isolation protection layer, and the service life of Comparative Example 1 is only 2.2 months. Comparative Example 2 does not inject oxygen into the silicon carbide film layer, and the service life of Comparative Example 2 is significantly reduced to 12.6 months. This shows the importance of setting an oxygen-containing silicon carbide film layer on the surface of the quartz part in the present application to improve the service life of the quartz part.
[0063] Further analyze the reasons.
[0064] The quartz parts in the LPCVD chamber are easy to break. The reason is that silicon is produced in the LPCVD process of Topcon battery production, which then adheres to the surface of the quartz parts and causes the quartz parts to break. For example, the quartz parts provided in Comparative Example 1 broke after a period of LPCVD process, and their service life was only 2.2 months.
[0065] In Comparative Example 2, a silicon carbide film is formed on the surface of the quartz part, and the silicon carbide film plays an isolating and protective role on the quartz part to prevent silicon from directly adhering. However, these silicon carbide films only play an isolating and protective role and cannot prevent the generation of silicon. After a period of use, some silicon will still adhere. The service life is only increased to 12.6 months compared with Comparative Example 1. This also shows that the traditional isolating and protective film layer has a limited effect on extending the service life of the quartz part.
[0066] Embodiment 1 forms an oxygen-containing silicon carbide film layer on the surface of the quartz piece. Firstly, it can play the role of a connecting layer between the quartz piece substrate and the attached impurities such as silicon oxide and silicon nitride generated after the process is used, so as to avoid the attached impurities generated after the process is used directly adhering to the quartz substrate to generate large internal stress, which will damage the quartz piece and cause cracks or breakage on the surface of the quartz piece. Specifically, Embodiment 1 forms an oxygen-containing silicon carbide film layer in advance by chemical vapor deposition before the battery production process is used, which can be well integrated with the surface of the quartz substrate and the attached impurities formed after the process is used, thereby avoiding the generation of internal stress. Secondly, the generation of silicon is the main reason for the damage to the quartz parts. The oxygen-containing silicon carbide film layer is formed on the surface of the quartz parts. In particular, compared with the comparative example 2, the embodiment 1 can prevent the generation of silicon during the process due to the injection of a large amount of oxygen elements, and other attached impurities, such as silicon nitride, silicon oxide, etc., can be dissolved in the surface of the quartz part with the silicon carbide layer set on the surface of the quartz part, and the internal stress generated on the surface of the quartz part is relatively small. Therefore, compared with the simple isolation protection film layer of the comparative example 2, the oxygen-containing silicon carbide film layer of the embodiment 1 can play a better role in extending the service life, which can be extended to 26.4 months.
[0067] (4) By comparing and analyzing Comparative Examples 3 to 4 with Example 1, it is shown that the flow ratio of the silicon source and oxygen in the process of injecting oxygen element affects the oxygen content, and thus affects the service life of the quartz parts. In Comparative Examples 3 and 4, the flow ratio of the silicon source and oxygen in the process of injecting oxygen element is 1:1 and 1:5 respectively. The service life of the quartz parts in Comparative Examples 3 and 4 is shortened to varying degrees. This shows that in the process of injecting oxygen element, the proportion of oxygen source in the silicon carbide raw material source should be within a certain range when the gas is introduced.
[0068] (5) The comparison between Comparative Examples 5 and 6 and Example 1 shows the effect of the thickness of the oxygen-containing silicon carbide film layer on the service life of the quartz part. The thicknesses of the oxygen-containing silicon carbide film layers of Comparative Examples 5 and 6 are 0.1 mm and 1.8 mm, respectively. The service life of the quartz parts of Comparative Examples 5 and 6 is shortened to varying degrees. This shows that the thickness of the silicon carbide film layer deposited on the surface of the quartz part needs to be controlled within a certain range. Combined with the analysis of Examples 1 to 5, the thickness is preferably 0.2 to 1.5 mm.
[0069] Further analyze the reasons.
[0070] Quartz parts are used in the LPCVD process involved in solar cell production. Therefore, most of their usage scenarios are high-temperature scenarios. If the thickness of the silicon carbide film is greater than 1.5 mm, the silicon carbide film layer will easily fall off after repeated alternations of high and low temperatures, and the service life of the quartz parts will be reduced. If the thickness of the silicon carbide film is less than 0.2 mm, the isolation protection effect is poor and the service life of the quartz parts will be reduced.
[0071] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for extending the service life of quartz parts, Features: The following steps are involved: Step S1: providing a quartz piece and placing it in a chemical vapor deposition chamber; Step S2: adjusting the pressure of the chamber to subnormal pressure, introducing a silicon source and a carbon source into the chamber, so as to deposit a silicon carbide film layer on the surface of the quartz piece; Step S3: adjusting the pressure of the chamber to 0.1-50 torr, and continuously introducing a silicon source and a carbon source into the chamber, and introducing an oxygen source into the chamber, so as to inject oxygen into the silicon carbide film layer on the surface of the quartz piece; wherein the introduction flow ratio of the silicon source to the oxygen source is 1:2-4; Step S4: taking the quartz piece out of the chemical vapor deposition chamber and putting it into production use.
2. A method for extending the service life of a quartz piece as claimed in claim 1, Features: In step S2, the sub-atmospheric pressure is 500-700 torr.
3. A method for extending the service life of a quartz piece as claimed in claim 1, Features: In step S2, the flow rate of the silicon source is 1-20 L / min, and the flow rate of the carbon source is 1-20 L / min.
4. A method for extending the service life of a quartz piece as claimed in claim 1, Features: In step S2, the silicon source and the carbon source are introduced for 10 to 40 minutes.
5. A method for extending the service life of a quartz piece as claimed in claim 1, Features: In step S3, the oxygen source is introduced for 5 to 20 minutes.
6. A method for extending the service life of a quartz piece as claimed in claim 1, Features: The thickness of the silicon carbide film layer is 0.2~1.5mm.
7. A method for extending the service life of a quartz piece as claimed in claim 1, Features: In steps S2 and S3, the temperature of the chamber is adjusted to 1200-1350°C.
8. A method for extending the service life of a quartz piece as claimed in claim 1, Features: The silicon source is monosilane and / or disilane.
9. A method for extending the service life of a quartz piece as claimed in claim 1, Features: The carbon source is propane and / or ethylene.
10. A method for extending the service life of a quartz piece as claimed in claim 1, Features: The oxygen source is oxygen gas.
Citation Information
Patent Citations
Quartz piece protective layer and preparation method thereof
CN113684468A
Quartz surface composite coating layer and preparation method thereof
CN113716878A
Quartz piece protective layer, preparation method thereof, modified quartz piece and application
CN117902835A
Cited By
Quartz tube matrix modification method based on multilayer structure melting hole sealing
CN122562347A