Wafer metallization structure, wafer metallization processing method and semiconductor structure

Through the partitioning and step-by-step method and cold spraying process, multiple metal blocks are formed on the wafer, and annealing and cleaning are performed, the problem of internal stress damage caused by adding metal layer with a thickness of more than 50μm on the wafer is solved, and the yield of the finished product is improved and connection strength improve the flow and heat dissipation performance of the wafer.

CN119050082APending Publication Date: 2024-11-29SHENZHEN PINGCHUANG SEMICON CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411230299.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to effectively increase the thickness of the metal layer greater than 50 μm on the wafer to avoid wafer damage caused by internal stress, especially the coating with a thickness greater than 10 μm may cause wafer damage, resulting in a low yield of the finished product.

Method used

The metal layer is deposited by a partitioning step method, and multiple metal blocks are formed on the wafer by cold spraying process, and annealing and cleaning are performed during the deposition process to improve the bond strength of the metal layer and the wafer and the finished product yield.

Benefits of technology

Through multiple deposition and annealing treatments, the stress caused by deposition is alleviated, the yield of finished products is improved, the risk of wafer warping is reduced, the connection strength between the metal layer and the wafer is enhanced, and the thickness is greater than 50μm but not more than 10μm is solved. The problem of metal layer causing wafer damage improves the flow and heat dissipation performance of the wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050082A_ABST
    Figure CN119050082A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductors, and particularly relates to a wafer metallization structure, a wafer metallization processing method and a semiconductor structure. The wafer metallization structure comprises a wafer and a metal layer deposited on the wafer, wherein the thickness of the metal layer is greater than 50 microns. The method solves the contradiction that the thickness of a metal layer added on the top of the wafer needs to be larger than 50 microns, but the thickness of the metal layer needs to be larger than 10 microns, so that the wafer is possibly damaged due to internal stress. According to the invention, the yield of finished products can be improved, and the through-flow performance, the heat dissipation performance and the reliability in the subsequent packaging process of the chip made of the wafer can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a wafer metallization structure, a wafer metallization processing method and a semiconductor structure. Background Art

[0002] As the power density of power electronic modules continues to increase, their operating temperature and current carrying capacity also increase, and the reliability issues caused by this are becoming increasingly severe. Current packaging materials have reached their application limits. Replacing aluminum bonding wires with copper bonding wires can improve the current carrying capacity, electrical conductivity, and thermal conductivity of the formed electronic components (or semiconductor devices), thereby increasing the life of the electronic components (or semiconductor devices).

[0003] However, there is usually only a thin layer of metal on the surface of the chip, and copper wires cannot be directly bonded. Usually, bonding copper wires requires a metal layer with a thickness of at least 50μm to ensure that the chip is not damaged. Wafer metallization is usually carried out by chemical plating or electroplating, which has high stress. A coating with a thickness greater than 10μm may cause the wafer to be damaged due to internal stress. Therefore, how to resolve the above contradictions has become a technical difficulty faced by technicians in this field.

[0004] In the related art, Heraeus proposed a method for manufacturing a device connected to a solder preform (publication number CN110741465A), comprising the following steps: (1) providing a device having at least one contact surface and a free solder preform; (2) manufacturing a configuration consisting of a device and a solder preform that has not yet been connected by bringing one or the only contact surface of the device into contact with a contact surface of the free solder preform; and (3) in the case of forming a device connected to the solder preform, hot pressing the configuration manufactured in step (2) at a temperature 10 to 40% lower than the melting temperature of the solder metal of the solder preform expressed in ° C, and under a combination of pressing pressure and pressing duration that reduces the initial thickness of the solder preform with initial freedom by ≤10%, that is, this scheme achieves interconnection with the chip by pre-coating metal solder on copper foil. However, when this method is used for processing, the solder and the copper foil are easily separated, the yield of the finished product is not high, and the pressurization will cause slippage between the solder and the copper foil, further reducing the yield and performance of the finished product.

[0005] Then Heraeus proposed a method for manufacturing a sandwich arrangement comprising a first component having a contact surface A, a second component having a contact surface D and a solder located between the contact surfaces A and D, wherein the method comprises: a fixing agent (consisting of the following components: 0 to 97 wt % (weight %) of at least one solvent selected from water and an organic solvent with a boiling point of ≤ 285°C, 3 to 100 wt % of at least one M1 material selected from (i) a thermoplastic organic polymer meltable between 30 and 180°C and (ii) a non-polymeric organic compound without an acidic group meltable between 30 and 180°C, 0 to 2 0% by weight of at least one M2 material selected from (iii) organic polymers which are not fusible between 30 and 180° C. and (iv) non-polymeric organic compounds which are not fusible between 30 and 180° C. and which have no acidic groups or have a boiling point higher than 285° C., and 0 to 30% by weight of one or more inorganic solid fillers, and wherein the sum of the surface areas of the contact surfaces A and B or C and D which together form a common overlapping area after the solder preform is placed, with the presence of one or more components (i) in the at least one M1 material, is 1500 μm 2 to 50 area % of the common overlapping area, and when only one or more components (ii) are present in the at least one M1 material, the sum is 1500 μm 2 To 100% of the common overlapping area) is applied to the contact surface A or D of the component to fix the preformed solder, then melted and the molten solder thus formed is cooled to below its solidification temperature, and a component with a solder deposit on its contact surface A or D is obtained, and the component is arranged with the free contact surface of its solder deposit facing the contact surface D or A of the component to be connected, wherein the fixing agent can be arranged between the contact surfaces to be connected, and then the solder deposit is melted and the molten solder thus obtained is cooled to below its solidification temperature, thereby forming a finished welding sandwich arrangement. However, the fixing agent raw material used in this scheme is a polymer material, which will affect the sintering of the solder, and the above two schemes are only for a single chip with a solderable surface, that is, a surface gold-plated or silver-plated material, and require specific mounting equipment (requires suction head heating and pressurization), and cannot solve the problem of wafer-level metallization. Obviously, the existing technology cannot well solve the contradiction between the thickness of the metal layer added on the top of the wafer needing to be greater than 50μm and the plating layer with a thickness greater than 10μm may cause the wafer to be damaged due to internal stress. Summary of the invention

[0006] In view of the shortcomings of the prior art mentioned above, the present invention provides a wafer metallization structure, a wafer metallization processing method and a semiconductor structure to solve the contradictory technical problem that the thickness of the metal layer added on the top of the above-mentioned wafer needs to be greater than 50μm, but the plating layer with a thickness greater than 10μm may cause damage to the wafer due to internal stress.

[0007] After studying the relevant technology, the inventors found that the prior art generally adopts a one-time deposition method to deposit the metal layer. However, when depositing the metal layer in this way, a coating with a thickness greater than 10μm may cause the wafer to be damaged due to internal stress, resulting in a low yield of the finished product.

[0008] To achieve the above objectives, the scheme of this application is as follows: In a first aspect, the present invention provides a wafer metallization structure, comprising a wafer and a metal layer deposited on the wafer, wherein the thickness of the metal layer is greater than 50 μm.

[0009] It should be noted that, in the present application, the metal layer is deposited on the top of the wafer.

[0010] Optionally, the metal layer consists of a plurality of metal blocks deposited on the wafer.

[0011] Optionally, the metal layer consists of 2n metal blocks deposited on the wafer, where n is a positive integer.

[0012] Optionally, all the metal blocks are deposited on the wafer in a zoned and step-by-step manner.

[0013] Optionally, the metal layer is deposited by using at least one of the following metals: copper, nickel, gold, silver, aluminum, ruthenium, cobalt and tin.

[0014] Optionally, the metal layer is deposited by using at least one of the following metal forms: spherical, polygonal and dendritic.

[0015] Optionally, the metal layer is formed by depositing metal particles with a particle size of 1-20 μm.

[0016] Optionally, the metal layer is formed by depositing metal particles with a plurality of different particle sizes and a particle size of 1-10 μm.

[0017] In a second aspect, the present invention provides a wafer metallization processing method, comprising the following steps: Preparing a metal layer on a wafer: adopting a zoned and step-by-step deposition method to prepare a plurality of metal blocks on the wafer to form the metal layer.

[0018] Optionally, a cold spraying process is used to prepare and form a plurality of metal blocks on the wafer.

[0019] Optionally, during the cold spraying process, the pressure is 2-4 MPa, preferably 2.5-4 MPa.

[0020] Optionally, during the cold spraying process, the working gas used is selected from at least one of nitrogen, helium, argon and neon.

[0021] Optionally, during the cold spraying process, the temperature of the working gas used is 100-300°C, preferably 150-300°C.

[0022] Optionally, during the cold spraying process, the spraying speed is 100-300 mm / s, preferably 150-300 mm / s.

[0023] Optionally, during the cold spraying process, the spraying distance is 10-30 mm, preferably 15-30 mm.

[0024] Optionally, in the process of preparing a plurality of metal blocks on the wafer by adopting the zoned and step-by-step deposition method, adjacent deposition processes further include: an annealing step.

[0025] Optionally, the annealing temperature is 200-350°C, preferably 250-350°C.

[0026] Optionally, the annealing time is 0.5-2 h, preferably 1-2 h.

[0027] Optionally, in the process of preparing a plurality of metal blocks on the wafer by adopting the zoned step-by-step deposition method, in the adjacent deposition process, after annealing, the following step is also included: cleaning the wafer.

[0028] Optionally, the wafer is cleaned by plasma.

[0029] Optionally, after the last annealing, the wafer is polished.

[0030] It should be noted that in the present application, each mask plate is provided with an opening, and the positions of the openings of different mask plates are different. The opening areas of all mask plates together constitute the target pattern, that is, the openings of each mask plate together constitute the target pattern in a form similar to building blocks, and the adjacent junctions of the opening areas of adjacent mask plates are crossed.

[0031] In a third aspect, the present invention further provides a semiconductor structure, comprising the wafer metallization structure as described above and / or a wafer metallization structure formed according to the method as described above.

[0032] Beneficial effects of the present invention: The present invention can alleviate stress caused by deposition through multiple depositions, thereby increasing deposition thickness and improving finished product yield.

[0033] The present invention can release the internal stress of the wafer through annealing treatment, thereby reducing the wafer warping, improving the finished product yield, and avoiding wafer breakage due to factors such as bonding and welding in subsequent processes.

[0034] The present invention deposits the metal layer by cold spraying, which can improve the bonding strength between the metal layer and the wafer. Compared with the second part of the electroplating method, the cold spraying method has smaller stress, thereby improving the bonding yield in the subsequent processing process and avoiding the separation of the metal layer and the wafer due to the bonding process.

[0035] The present invention deposits a metal layer using a single metal or a mixture of different metal single substances, thereby increasing the density of the metal layer, increasing the connection area with the wafer surface, and further improving the bonding strength between the metal layer and the wafer.

[0036] In the present invention, the wafer is cleaned before the metal layer is deposited, so that the connection strength between the wafer and the metal layer can be improved.

[0037] In the present invention, the metal layer formed by metal particles with different particle sizes within the particle size range of 1-10 μm can further improve the connection strength between the metal layer and the wafer.

[0038] The invention improves the yield rate of finished products.

[0039] The present invention solves the contradiction that the thickness of the metal layer added on the top of the wafer needs to be greater than 50 μm, but a plating layer with a thickness greater than 10 μm may cause the wafer to be damaged due to internal stress.

[0040] The present invention can improve the flow performance and heat dissipation performance of the chip made of the wafer as well as the reliability in the subsequent packaging process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A schematic diagram of a mask plate used in Examples 1-3; Figure 2 Schematic diagram of the metal layer formed after multiple depositions in Examples 1-3.

[0042] Figure 3 This is the relationship diagram between spraying speed and connection strength; Figure 4 The relationship between cleaning and connection strength is shown in the figure; Figure 5 is the relationship between the particle size of metal particles and the connection strength; Figure 6 It is a schematic diagram of the chip + metal layer + bonding wire structure; Figure 7 Schematic diagram of chip + bonding wire structure. DETAILED DESCRIPTION

[0043] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0044] An embodiment of the present invention provides a wafer metallization structure, including a wafer and a metal layer deposited on the wafer, the thickness of the metal layer is greater than 50 μm, the metal layer is composed of 2n metal blocks deposited on the wafer, n is a positive integer, all metal blocks are deposited on the wafer using a zoned step method, the metal layer is deposited using at least one of the following metals: copper, nickel, gold, silver, aluminum, ruthenium, cobalt and tin, the metal layer is deposited using at least one of the following metal forms: spherical, polygonal and dendritic, and the metal layer is deposited using metal particles with a particle size of 1-20 μm.

[0045] In another embodiment of the present invention, the metal layer is formed by depositing metal particles with a plurality of different particle sizes and a particle size of 1-10 μm.

[0046] Another embodiment of the present invention provides a wafer metallization processing method, comprising the following steps: Preparing a metal layer on a wafer: using a zoned step-by-step deposition method to prepare and form a plurality of metal blocks on the wafer to form a metal layer, and using a cold spraying process to prepare and form a plurality of metal blocks on the wafer.

[0047] Another embodiment of the present invention further provides a semiconductor structure, comprising the wafer metallization structure as described above and / or a wafer metallization structure formed according to the method as described above.

[0048] The following specific examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range according to the description herein, and are not limited to the specific values ​​​​exemplified below.

[0049] It should be understood that in the following embodiments, only copper, silver and aluminum are listed as specific cases of metals, and those skilled in the art may also choose other metals besides copper, aluminum and silver, such as nickel, gold, ruthenium, cobalt, tin, etc., or a mixture of at least two of the metals selected from copper, silver, aluminum, gold, ruthenium, cobalt and tin.

[0050] Example 1 A wafer metallization processing method, the specific steps are as follows: Place the first mask on top of the wafer (such as Figure 1 As shown in the leftmost figure), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the first mask and anneal at 300°C for 1h; Place the second mask on the wafer (such as Figure 1 As shown in the second figure from left to right), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the second mask and anneal at 300℃ for 1h... Repeat this cycle 4 times. The parameters are set exactly the same during the 4 cycles. Then polish and grind. The resulting pattern is as follows: Figure 2 As shown; During the cold spraying process, the metal is selected from copper particles (spherical) with a particle size of 1μm. During the cold spraying process, the working gas used is selected from nitrogen. The temperature of the working gas used is 100°C, the pressure is 2MPa, the spraying speed is 100mm / s, and the spraying distance (that is, the distance between the nozzle used and the wafer, the nozzle used is a Laval nozzle) is 30mm.

[0051] In this embodiment, the thickness of the first mask is 105 μm, and the thickness of the second mask, the third mask, and the fourth mask are all 10 μm.

[0052] In this embodiment, each mask plate is provided with an opening, and the positions of the openings of different mask plates are different. The opening areas of all mask plates together constitute the target pattern, that is, the openings of each mask plate together constitute the target pattern in a form similar to laying floor tiles, and the adjacent intersections of the opening areas of each mask plate are crossed.

[0053] Example 2 A wafer metallization processing method, the specific steps are as follows: Place the first mask on top of the wafer (such as Figure 1 As shown in the leftmost figure), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the first mask and anneal at 300°C for 1h; Place the second mask on the wafer (such as Figure 1 As shown in the second figure from left to right), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the second mask and anneal at 300℃ for 1h... Repeat this cycle 4 times. The parameters are set exactly the same during the 4 cycles. Then polish and grind. The resulting pattern is as follows: Figure 2 As shown; During the cold spraying process, the metal is selected from silver particles (polygonal) with a particle size of 10μm. During the cold spraying process, the working gas used is selected from nitrogen. The temperature of the working gas used is 100°C, the pressure is 4MPa, the spraying speed is 300mm / s, and the spraying distance (that is, the distance between the nozzle used and the wafer, the nozzle used is a Laval nozzle) is 30mm.

[0054] In this embodiment, the thickness of the first mask is 55 μm, and the thickness of the second mask, the third mask, and the fourth mask are all 10 μm.

[0055] Example 3 A wafer metallization processing method, the specific steps are as follows: Place the first mask on top of the wafer (such as Figure 1 As shown in the leftmost figure), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the first mask and anneal at 200°C for 2h; Place the second mask on the wafer (such as Figure 1 As shown in the second figure from left to right), the wafer is cleaned by plasma; Depositing the metal layer by cold spraying; Remove the second mask and anneal at 200℃ for 2h... Repeat this cycle 4 times. The parameters are set exactly the same during the 4 cycles. Then polish and grind. The resulting pattern is as follows: Figure 2 As shown; During the cold spraying process, the metal is selected from silver particles (polygonal) with a particle size of 20μm. During the cold spraying process, the working gas used is selected from nitrogen. The temperature of the working gas used is 200°C, the pressure is 3MPa, the spraying speed is 150mm / s, and the spraying distance (that is, the distance between the nozzle used and the wafer, the nozzle used is a Laval nozzle) is 10mm.

[0056] In this embodiment, the thickness of the first mask is 75 μm, and the thickness of the second mask, the third mask, and the fourth mask are all 10 μm.

[0057] Example 4 The difference between this embodiment and embodiment 1 is that the spraying speed is 150 mm / s.

[0058] Example 5 The difference between this embodiment and embodiment 1 is that the spraying speed is 200 mm / s.

[0059] Example 6 The difference between this embodiment and embodiment 1 is that the spraying speed is 250 mm / s.

[0060] Example 7 The difference between this embodiment and embodiment 1 is that the spraying speed is 300 mm / s.

[0061] Example 8 The difference between this embodiment and Embodiment 1 is that the wafer is not cleaned before depositing the metal layer.

[0062] Example 9 The difference between this embodiment and embodiment 1 is that the particle size of the copper particles is 10 μm.

[0063] Example 10 The difference between this embodiment and embodiment 1 is that the particle size of the copper particles is 20 μm.

[0064] Embodiment 11 The difference between this embodiment and embodiment 1 is that the metal is a mixture of copper particles with a particle size of 1 μm and copper particles with a particle size of 10 μm in a mass ratio of 1:1.

[0065] Example 12 The difference between this embodiment and the first embodiment is that the thickness of the first mask is 55 μm, and the thickness of the second mask, the third mask and the fourth mask are all 10 μm.

[0066] Embodiment 13 The difference between this embodiment and Embodiment 2 is that the thickness of the first mask is 75 μm, and the thickness of the second mask, the third mask and the fourth mask are all 10 μm.

[0067] Embodiment 14 The difference between this embodiment and Embodiment 2 is that the thickness of the first mask is 105 μm, and the thicknesses of the second mask, the third mask and the fourth mask are all 10 μm.

[0068] Embodiment 15 The difference between this embodiment and the first embodiment is that the thickness of the first mask is 55 μm, the thickness of the second mask, the third mask and the fourth mask are all 10 μm; and aluminum particles with a particle size of 1 μm are used to replace copper particles with a particle size of 1 μm.

[0069] Example 16 The difference between this embodiment and Embodiment 15 is that the thickness of the first mask is 75 μm, and the thickness of the second mask, the third mask and the fourth mask are all 10 μm.

[0070] Embodiment 17 The difference between this embodiment and Embodiment 15 is that the thickness of the first mask is 105 μm, and the thickness of the second mask, the third mask and the fourth mask are all 10 μm.

[0071] Comparative Example 1 The difference between this comparative example and Example 1 is that: a first mask is mounted on the wafer, and the opening size and shape of the first mask are as follows: Figure 2 As shown in the white area in the middle, the wafer is cleaned by plasma; The metal layer is deposited by cold spraying. The metal is selected from copper particles with a particle size of 1 μm. During the cold spraying process, the working gas used is selected from nitrogen. The temperature of the working gas used is 100°C, the pressure is 2 MPa, the spraying speed is 100 mm / s, and the spraying distance (that is, the distance between the nozzle used and the wafer, the nozzle used is a Laval nozzle) is 30 mm.

[0072] That is, this comparative example adopts a one-time deposition method rather than a multiple-time deposition method.

[0073] Comparative Example 2 The difference between this comparative example and Example 1 is that no annealing treatment is performed after the metal layer is deposited.

[0074] Comparative Example 3 The difference between this comparative example and Example 1 is that the metal layer is deposited by electroplating instead of cold spraying, the electrolyte is a copper sulfate solution with a concentration of 50g / L, and the current density is 5Ma / cm 2 .

[0075] Comparative Example 4 The difference between this comparative example and Example 1 is that copper oxide particles with a particle size of 1 μm are used instead of copper particles with a particle size of 1 μm.

[0076] test The thickness of the deposited metal layer of Examples 1-17 and Comparative Examples 1-3 was detected, and several finished products were prepared according to the methods of Examples 1-11 and Comparative Examples 1-3, respectively. The damage of the wafers after treatment was observed, and the yield of the finished products was counted. The results are shown in Table 1; The connection strength between the wafer and the metal layer after the treatment of Examples 1-11 and Comparative Examples 1-3 was tested, and the results are shown in Tables 1 and Figures 3 to 5 As shown; Among them, the thickness of the metal layer is detected by a coating thickness gauge; The connection strength test method is: slice the wafer, push the metal protrusions on the wafer surface with a table-top push-pull force device, and test the connection strength.

[0077] Table 1 Thickness, damage, yield and connection strength test results

[0078] As shown in Table 1, in Examples 1-3, the thickness of the metal layer was ≥50 μm, the wafer was not damaged, and the yield was greater than 99%. This result shows that the method of the present invention solves the contradiction that the thickness of the metal layer added on the top of the wafer needs to be greater than 50 μm, but the plating layer with a thickness greater than 10 μm may cause the wafer to be damaged due to internal stress.

[0079] From Table 1 and Figure 3 It can be seen that within the spraying speed range of 100-300 m / s, as the spraying speed increases, the connection strength between the wafer and the metal layer increases. This result shows that in the present invention, within the spraying speed range of 100-300 m / s, increasing the spraying speed helps to improve the connection strength between the wafer and the metal layer, but the yield rate decreases.

[0080] From Table 1 and Figure 5 It can be seen that within the range of 1-20 μm of metal particle size, as the particle size increases, the bonding strength between the wafer and the metal layer first increases and then decreases; compared with Example 1 (the metal is selected from copper particles of a single particle size), the connection strength between the metal layer and the wafer in Example 11 (the metal is selected from a mixture of copper particles with a particle size of 1 μm and copper particles with a particle size of 10 μm in a mass ratio of 1:1) increases significantly. This result shows that the metal layer formed by metal particles of different particle sizes within the particle size range of 1-10 μm can further improve the connection strength between the metal layer and the wafer.

[0081] From Table 1 and Figure 4 It can be seen that compared with Example 8 (the wafer was not cleaned before the metal layer was deposited), the connection strength between the wafer and the metal layer in Example 1 (the wafer was cleaned before the metal layer was deposited) was significantly increased. This result shows that in the present invention, cleaning the wafer before depositing the metal layer can improve the connection strength between the wafer and the metal layer.

[0082] As can be seen from Table 1, compared with Example 1 (the metal is selected from copper particles with a particle size of 1 μm), the bonding strength of Example 11 (the metal is a mixture of copper particles with a particle size of 1 μm and copper particles with a particle size of 10 μm in a mass ratio of 1:1) is significantly improved. This result shows that the metal layer formed by metal particles of different particle sizes within the particle size range of 1-10 μm in the present invention can increase the density of particle accumulation, thereby improving the bonding strength between the metal layer and the wafer.

[0083] As shown in Table 1, compared with Example 8 (the wafer was not cleaned before the metal layer was deposited), the bonding strength of Example 1 (the wafer was cleaned before the metal layer was deposited) was significantly improved. This result shows that in the present invention, cleaning the wafer before depositing the metal layer can improve the connection strength between the wafer and the metal layer.

[0084] As shown in Table 1, the yield of Comparative Example 1 (using a single deposition method) is 79%, while the yield of Example 1 (using multiple deposition methods) is 99%. This result shows that the present invention can relieve the stress caused by deposition through multiple depositions, thereby increasing the deposition thickness and improving the yield of the finished product.

[0085] As can be seen from Table 1, compared with Comparative Example 2 (without annealing treatment), the yield of Example 1 (after annealing treatment) is significantly increased. This result shows that the present invention can release the internal stress of the wafer through annealing treatment, thereby reducing the wafer warpage, improving the yield of the finished product, and avoiding wafer breakage due to factors such as bonding and welding in the subsequent process.

[0086] As shown in Table 1, compared with Comparative Example 3 (depositing the metal layer by electroplating), the bonding strength of Example 1 (depositing the metal layer by cold spraying) is significantly increased. This result shows that the present invention can improve the bonding strength between the metal layer and the wafer by depositing the metal layer by cold spraying.

[0087] As can be seen from Table 1, compared with Comparative Example 4 (using copper oxide particles), the connection strength of Example 1 (using copper particles) is significantly improved. This result shows that the present invention can improve the bonding strength between the metal layer and the wafer by depositing the metal layer using a single metal or a mixture of different metal single substances.

[0088] The finished products of Examples 1-3 and Examples 12-17 were cut into chips respectively, and the maximum junction temperature of the chips was tested. The results are shown in Table 2. The test method for the maximum junction temperature of the chip is: using the comsol software to establish the bonding model of the chips cut from the wafers after the processing of Examples 1-3 and Examples 12-17 and different bonding wires (such as Figure 6 ), and use the software to establish a bonding model between a chip cut from a separate unprocessed wafer from the same source as in Example 1 and an aluminum wire (such as Figure 7 As shown in the figure, the chip thickness is 0.12μm, the solder layer thickness at the bottom of the chip is 0.1μm, the material is tin, the substrate is made of copper, the difference between the top of the chip and whether a metal layer is used, the bonding wire material is copper or aluminum, and the bonding wire diameter is 15mil. The chip is set as a heat source and works continuously with a fixed loss of 50W. The copper substrate is set as a convection heat transfer boundary, and the other surfaces are insulation surfaces. Comsol software is used to calculate the maximum surface temperature of the chip (i.e., the maximum junction temperature of the chip). The results are shown in Table 2.

[0089] Table 2 Chip maximum junction temperature test results

[0090] As shown in Table 2, the maximum junction temperature of the chip in Examples 1-3 and Examples 12-17 is less than 70° C., while the maximum junction temperature of the chip in the aluminum wire control group is greater than 70° C. This result shows that the method of the present invention can improve the flow performance and heat dissipation performance of the chip made of the wafer and the reliability in the subsequent packaging process.

[0091] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A wafer metallization structure, characterized in that: The invention comprises a wafer and a metal layer deposited on the wafer, wherein the thickness of the metal layer is greater than 50 μm.

2. The wafer metallization structure according to claim 1, characterized in that: The metal layer is composed of a plurality of metal blocks deposited on the wafer.

3. The wafer metallization structure according to claim 2, characterized in that: The metal layer is composed of 2n metal blocks deposited on the wafer, where n is a positive integer.

4. The wafer metallization structure according to claim 2, characterized in that: All the metal blocks are deposited on the wafer in a zone-by-zone step-by-step manner.

5. The wafer metallization structure according to claim 1, characterized in that: The metal layer is deposited by using at least one of the following metals: copper, nickel, gold, silver, aluminum, ruthenium, cobalt and tin.

6. The wafer metallization structure according to claim 1, characterized in that: The metal layer is formed by depositing metal particles with a particle size of 1-20 μm; And / or, the metal layer is deposited by using at least one of the following metal forms: spherical, polygonal and dendritic.

7. The wafer metallization structure according to claim 6, characterized in that: The metal layer is formed by depositing metal particles with various particle sizes of 1-10 μm.

8. A wafer metallization processing method, characterized in that: The following steps are involved: Preparing a metal layer on a wafer: adopting a zoned and step-by-step deposition method to prepare a plurality of metal blocks on the wafer to form the metal layer.

9. The wafer metallization processing method according to claim 8, characterized in that: A cold spraying process is adopted to prepare and form a plurality of metal blocks on the wafer.

10. A semiconductor structure, characterized in that: It comprises the wafer metallization structure according to any one of claims 1 to 7 and / or the wafer metallization structure formed according to the method of claim 8 or 9.

Citation Information

Patent Citations

  • Method for isolated and discretized process sequence integration

    CN102148134A

  • Semiconductor device and method for manufacturing the same

    CN102549738A

  • Method for Producing a Copper Layer on a Semiconductor Body Using a Printing Process

    CN104810247A

  • Top layers of metal for high performance IC's

    US20040166659A1