Silicon carbide-based hybrid diode and preparation method thereof

By increasing the ohmic contact area and improving the electric field distribution in the silicon carbide-based hybrid diode, the problems of uneven current distribution and insufficient reverse voltage due to small ohmic contact area of ​​traditional MPS are solved, and the thermal stability and reliability of the device are improved sex.

CN119050161APending Publication Date: 2024-11-29SHENZHEN BASIC SEMICON LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411001605.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to the small ohmic contact area of ​​traditional silicon carbide hybrid diodes (MPS), the current distribution is uneven, local overheating and electromigration problems, affecting the reliability and life of the device, and insufficient reverse voltage withstand voltage.

Method used

During the preparation of silicon carbide-based hybrid diodes, an ohmic contact groove is formed by growing an N-type epitaxial layer on an N-type silicon carbide substrate and forming an ohmic metal layer on its front and back side, injecting P-type impurities, etching to form an ohmic contact groove and Filling ohmic metals, increasing the contact area, combining Schottky grooves to form Schottky barriers, increasing the contact area and improving the electric field distribution.

Benefits of technology

By increasing the ohmic contact area, the current distribution is more uniform, reducing the risks of thermal aggregation and electromigration, improving the thermal stability and reliability of the device, and enhancing the reverse withstand voltage, able to withstand greater forward transient currents and High reverse breakdown voltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050161A_ABST
    Figure CN119050161A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of chips, and discloses a silicon carbide hybrid diode and a preparation method thereof, and the preparation method comprises the steps: obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating an ohmic metal layer on the back surface of the N-type silicon carbide substrate; injecting P-type impurities into a first active region of a cellular region of the N-type epitaxial layer to generate a first P-type doped region; an ohmic contact groove is formed in the first active region through etching by means of a photoetching process, and the ohmic contact groove is located in the first P-type doped region; the ohmic contact groove is filled with ohmic metal; and sputtering Schottky metal on the surface of the second active region in the cellular region. By using the method disclosed by the invention, a series of problems caused by small ohmic contact area of the traditional MPS in the prior art can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chips and relates to a silicon carbide-based hybrid diode and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC), as a typical representative of the third generation of semiconductors, not only has a wide bandgap, but also has advantages such as high breakdown voltage, high thermal conductivity, and high electron saturation rate. Therefore, power electronic devices made of silicon carbide materials have higher withstand voltage, greater current carrying capacity, and higher operating frequency, and can work in high-frequency and high-temperature environments with high reliability, and can be suitable for harsh working environments. Therefore, silicon carbide materials, as third-generation power electronic devices, have become the most important development direction of power electronic technology, and have important application prospects in military and civil fields.

[0003] In silicon carbide diodes, the significant advantages of the Schottky structure are fast switching speed, being a majority carrier device, and having no reverse recovery time. However, under high voltage, the Schottky barrier degenerates, the reverse leakage is large, and the high voltage resistance characteristic cannot be achieved. Compared with the Schottky structure, the Positive-Intrinsic-Negative (PiN) device has a higher withstand voltage, but a longer reverse recovery time and a larger forward voltage drop. The Junction Barrier Schottky diode (JBS) is a device structure that combines the Schottky and PiN structures, combining the advantages of both, with high voltage, low leakage, low forward conduction voltage reduction, and fast reverse recovery time.

[0004] Usually, a silicon carbide hybrid diode (Metal-PIN-Schottky Diode, MPS) has an additional layer of photolithography on the basis of the traditional JBS, so that the ohmic metal and Schottky metal are made separately, thereby reducing the ohmic contact resistance and improving the forward surge capability.

[0005] However, in traditional MPS, the P+ ohmic contact is only implemented on the surface of the silicon wafer, which limits the current distribution and the thermal performance of the device. When current passes through this structure, due to the limited contact area, the current density may be very high at the contact point, causing local overheating and electromigration problems, thus affecting the reliability and life of the device. In addition, the small contact area may also limit the forward surge current capability and make the reverse withstand voltage insufficient. Summary of the invention

[0006] The present invention provides a silicon carbide hybrid diode and a preparation method thereof, which are used to solve a series of problems caused by the small ohmic contact area of ​​the traditional MPS in the prior art.

[0007] In order to solve the above technical problems, in a first aspect, the present invention provides a method for preparing a silicon carbide-based hybrid diode, comprising:

[0008] Obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating an ohmic metal layer on the back surface of the N-type silicon carbide substrate;

[0009] Injecting P-type impurities into a first active region of a cell region of the N-type silicon carbide epitaxial layer to generate a first P-type doped region;

[0010] Etching an ohmic contact groove in the first active region by a photolithography process, wherein the ohmic contact groove is located in the first P-type doped region;

[0011] Filling the ohmic contact groove with ohmic metal;

[0012] A Schottky metal is sputtered on the surface of the second active region in the cell region.

[0013] Optionally, after etching the ohmic contact trench in the first active region by a photolithography process and before filling the ohmic contact trench with an ohmic metal, the method further includes:

[0014] P-type impurities are implanted into the bottom of the ohmic contact trench to form a P-type impurity barrier at the bottom of the ohmic contact trench.

[0015] Optionally, the sputtering of Schottky metal on the surface of the second active region in the cell region includes:

[0016] Etching a Schottky trench on the surface of the second active region;

[0017] A Schottky metal is sputtered in the Schottky trench, and the Schottky metal is alloyed with silicon carbide to form a Schottky barrier.

[0018] Optionally, after growing an N-type epitaxial layer on the front surface of the N-type silicon carbide substrate and before etching to form an ohmic contact trench in the first active region by a photolithography process, the method further includes:

[0019] P-type impurities are implanted into the terminal region of the cell region of the N-type silicon carbide epitaxial layer to generate a second P-type doped region.

[0020] Optionally, a doping concentration of the P-type impurity barrier is greater than a doping concentration of the first P-type doping region.

[0021] Optionally, a width of the first P-type doping region is greater than a width of the second P-type doping region.

[0022] Optionally, the P-type impurity is aluminum.

[0023] Optionally, etching the ohmic contact groove in the first active region by a photolithography process includes:

[0024] Depositing LPTEOS as a barrier layer on the surface of the cell region;

[0025] Sputtering nickel on the LPTEOS as an etching shielding layer;

[0026] Etching the shielding layer and the blocking layer by a photolithography process, and removing the photoresist after the etching is completed;

[0027] The exposed surface of the cell region is etched to form an ohmic contact groove.

[0028] Optionally, the Schottky metal is titanium.

[0029] In a second aspect, the present invention provides a silicon carbide-based hybrid diode, comprising:

[0030] N-type silicon carbide substrate;

[0031] An ohmic metal layer is formed on the back side of the N-type silicon carbide substrate;

[0032] An N-type silicon carbide epitaxial layer is grown on the front surface of the N-type silicon carbide substrate, and an ohmic contact groove is etched in the first active region of the cell region, and a Schottky groove is etched in the second active region of the cell region;

[0033] A Schottky metal is formed on the surface of the Schottky trench;

[0034] Ohmic metal, filled in the ohmic contact groove;

[0035] A first P-type doped region is located in a first active region of a cell region of the N-type silicon carbide epitaxial layer, and the ohmic contact trench is located in the first P-type doped region;

[0036] A P-type impurity barrier is formed at the bottom of the ohmic contact trench, and the doping concentration of the P-type impurity barrier is greater than the doping concentration of the first P-type doping region;

[0037] The second P-type doped region is located in the terminal region of the N-type silicon carbide epitaxial layer.

[0038] Compared with the prior art, the method for preparing a silicon carbide-based hybrid diode provided by the present invention has the following beneficial effects:

[0039] In the process of preparing a silicon carbide-based hybrid diode, the present invention etches an ohmic contact groove in the first P-type doped region, and fills the ohmic contact groove with an ohmic metal, so that in the first P-type doped region, the P-type impurities that make ohmic contact with the ohmic metal can be located on the two side walls and the bottom silicon surface of the first P-type doped region, so that the ohmic contact area of ​​the P-type impurities in the first P-type doped region can be greatly increased, and the increase in the contact area means that the current can be more evenly distributed over a larger area, which reduces the local current density, reduces the risk of heat accumulation and electromigration, and thus improves the thermal stability and reliability of the device; and because the contact area is increased, the device can withstand a larger forward transient current without overheating or damage, which is particularly important for applications that need to handle large currents; in addition, the reverse withstand voltage can be improved, because the reverse ohmic metal is used as a field plate, which can improve the electric field distribution and increase the reverse breakdown voltage of the device, which means that under reverse bias conditions, the device can withstand a higher voltage without being broken down. In summary, the present invention can solve a series of problems caused by the small ohmic contact area of ​​the traditional MPS in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present invention, rather than all of the embodiments. For ordinary technicians in this field, without paying creative work, other drawings obtained based on these drawings all fall within the scope of protection of this application.

[0041] Figure 1 It is a flow chart of a method for preparing a silicon carbide-based hybrid diode provided by an embodiment of the present invention;

[0042] Figures 2 to 12 It is a structural schematic diagram corresponding to the preparation process of the silicon carbide-based hybrid diode provided by an embodiment of the present invention;

[0043] Fig.13 It is a schematic diagram of the structure of a silicon carbide-based hybrid diode provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] In order to make the description of the disclosed content more detailed and complete, the following is an illustrative description of the implementation mode and specific examples of the present invention; however, this is not the only form of implementing or applying the specific embodiments of the present invention. The implementation mode covers the features of multiple specific embodiments and the method steps and their sequence for constructing and operating these specific embodiments. However, other specific embodiments can also be used to achieve the same or equal functions and step sequences. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0046] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.

[0047] In addition, in the description of the embodiments of the present application, "multiple" refers to two or more than two, and other quantifiers are similar and should be understood. The preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. In addition, the embodiments of the present application and the features therein may be combined with each other if there is no conflict.

[0048] like Figure 1 Shown is a flow chart of a method for preparing a silicon carbide-based hybrid diode provided by an embodiment of the present invention, which includes the following steps.

[0049] Step S101 : obtaining an N-type silicon carbide substrate 100 , growing an N-type silicon carbide epitaxial layer 200 on the front surface of the N-type silicon carbide substrate 100 , and generating an ohmic metal layer 300 on the back surface of the N-type silicon carbide substrate.

[0050] The structure generated in this step is as follows Figure 2 shown.

[0051] It should be noted that the N-type silicon carbide substrate 100 refers to an N-type semiconductor formed by doping N-type impurity atoms (such as nitrogen or phosphorus) into silicon carbide material;

[0052] The N-type silicon carbide epitaxial layer 200 is a layer of N-type semiconductor material deposited on the N-type silicon carbide substrate 100 by epitaxial growth technology, wherein a gas containing a nitrogen source (N-type dopant) reacts with a gas containing a carbon source and a silicon source at a high temperature and is deposited on the substrate to form an epitaxial layer. N-type dopants (such as nitrogen or phosphorus) are introduced during the growth process to ensure that the material has sufficient free electrons, thereby exhibiting the electrical characteristics of an N-type semiconductor.

[0053] Optionally, the thickness of the N-type silicon carbide substrate 100 may be 300-400 um (micrometers), because if the thickness of the substrate is too thin, it is easy to break during the preparation process, and if the thickness of the substrate is too thick, it will cause waste. The doping concentration of the substrate may be greater than 1e19 / cm 3 (cubic centimeters) to ensure sufficiently low resistance.

[0054] It should be noted that the doping concentration of the N-type silicon carbide epitaxial layer 200 must be lower than the doping concentration of the N-type silicon carbide substrate 100 because the substrate is used for conducting and does not withstand voltage. Therefore, the epitaxial layer needs to have a lower doping concentration to withstand voltage.

[0055] Optionally, the doping concentration of the N-type silicon carbide epitaxial layer 200 may be 1e15-1e16 / cm 3 , the thickness can be between 10-12um.

[0056] It should be noted that the method of generating the ohmic metal layer 300 on the back side of the N-type silicon carbide substrate 100 may be any achievable method;

[0057] As a specific example, an ohmic metal (such as titanium, nickel or silver) may be sputtered or evaporated on the back side of the N-type silicon carbide substrate 100 to form an ohmic contact, and the back side thickness may be reduced to 100-200 um.

[0058] Step S102 , implanting P-type impurities into a first active region of a cell region of the N-type silicon carbide epitaxial layer to generate a first P-type doped region 410 .

[0059] The specific structure generated in this step is as follows Figure 3 shown.

[0060] Optionally, the P-type impurity injected in this step may be aluminum.

[0061] Optionally, in the process of injecting P-type impurities in this step, the injection may be performed multiple times with different concentrations to form a first P-type doping region 410 with a concentration gradient. The first P-type doping region 410 may be called a P+ column. As a specific example, the number of injections of P-type impurities may be 3 to 5 times, and the energy of the first injection of P-type impurities is 30-40kev (kiloelectron volts) and the dose is 1-5e15 / cm 3 The energy of the second injection of P-type impurities is 80-120keV, and the dose is 1-5e13 / cm 3 The third injection energy is 200-300kev and the dose is 15e13 / cm 3 The fourth injection energy is 300-400kev and the dose is 1-5e14 / cm 3The fifth implantation energy is 400-500kev and the dose is 1-5e15 / cm 3 , and the injection temperature of P-type impurities can be at a high temperature of 500-600°C.

[0062] Optionally, the number of the first P-type doping regions 410 may be multiple, for example, three, and the width and spacing of the multiple first P-type doping regions 410 may be specifically set according to application needs, for example, the width may be 1-2um, and the spacing may be 2-4um.

[0063] Specifically, Figure 3 As shown, before the P-type impurities are implanted, an implantation region may be formed by etching on the top surface of the epitaxial layer through a photolithography process. As a specific example, after the epitaxial layer is cleaned, a sandwich structure hard mask (HM) is grown on the top surface of the epitaxial layer, wherein the first layer of the HM may be a thermal oxide layer 411padox, and the thickness may be 400-500A (angstroms). This thermal oxide layer may be used as a shielding layer when P-type impurities are injected, and the thickness uniformity of the thermal oxide layer is better controlled. The second layer may be a polysilicon layer 412, and this layer may be used as a transition layer, and this layer may be used to connect the first layer and the third layer, so that the endpoint detection signal is strong during etching. The third layer may be low pressure tetraethoxysilane 413 (Low Pressure TetraEthyl OrthoSilicate, LPTEOS), and the thickness may be 2-2.5um. It may be further subjected to high temperature densification, and then photolithography patterning may be performed, and operations of coating, exposure and development may be performed. The thickness of the photoresist may be 2-2.5um, and then etching may be started. Etching may be performed using an inductively coupled plasma (ICP) with better anisotropy. Plasma, ICP) or transverse capacitively coupled plasma (TCP) plasma dry etching is performed, firstly etching the top LPTEOS413, stopping at the polysilicon layer 412, then etching the polysilicon layer 412, stopping at the pad ox411, then removing the glue and cleaning to form an implantation area.

[0064] Step S103 , etching to form an ohmic contact trench 500 in the first active region by a photolithography process.

[0065] The ohmic contact trench 500 is located in the first P-type doping region 410 .

[0066] The specific structure generated in this step is as follows Figure 4 shown.

[0067] It should be noted that the method of etching the ohmic contact groove 500 in the first active region by the photolithography process in this step can be any achievable method. As a specific example, in this step, the hard mask layer in step S102 can be first removed, and then the region to be etched can be re-formed by the photolithography process. The region to be etched must be located in the implantation region of the first P-type doped region 410, so that the ohmic contact groove 500 is located in the first P-type doped region 410. After the region to be etched is formed, the region to be etched is etched;

[0068] As a specific example, the etching method for etching the area to be etched may be dry etching, the etching depth may be 0.8-1.2 um, and the width may be 0.8-1.2 um.

[0069] Step S104 , filling the ohmic contact trench 500 with an ohmic metal 510 .

[0070] The specific structure generated in this step is as follows Figure 5 shown.

[0071] Before this step, the epitaxial layer may be activated at a high temperature, for example, the activation temperature may be 1600-1750 degrees Celsius and the activation time may be 20-30 minutes;

[0072] Optionally, in order to prevent the surface of the epitaxial layer from becoming rough after the high-temperature reaction, which makes subsequent processes impossible to process, a carbon film 520 can be sputtered on the surface of the epitaxial layer before high-temperature activation, and the carbon film 520 can be removed after the high-temperature reaction. Figure 6 shown.

[0073] It should be noted that the ohmic metal 510 filled in this step may be nickel, gold or tantalum, etc., which is not limited in detail here;

[0074] As a specific example, the thickness of the ohmic metal 510 filled in the ohmic contact trench 500 can be 0.5-0.8um, and the ohmic metal 510 at the top of the ohmic contact trench 500 can be further removed by a chemical mechanical polishing (CMP) process so that the thickness of the ohmic metal 510 remains level with the top of the ohmic contact trench 500.

[0075] It should be noted that after this step, the ohmic metal 510 is filled in the ohmic contact groove 500, so that the ohmic metal 510 can be alloyed with the silicon carbide in the ohmic contact groove 500. To ensure that the ohmic metal 510 and silicon carbide are smoothly alloyed, the ohmic metal 510 and silicon carbide can be reacted at 550-750°C (degrees Celsius) for 10-20 minutes.

[0076] Step S105 , sputtering a Schottky metal 600 on the surface of the second active region in the cell region.

[0077] Specific structure such as Figure 7 shown.

[0078] It should be noted that after the Schottky metal 600 is sputtered on the surface of the second active region in this step, the Schottky metal 600 and the silicon carbide surface can form a Schottky alloy, and finally form a Schottky barrier.

[0079] Optionally, after this step, a top metal 700 may be sputtered on the top layer, such as aluminum, and the thickness of the sputtered aluminum may be 3-4 um, etc. The specific structure is as follows: Figure 8 shown.

[0080] Optionally, after this step, a passivation layer 800 may be formed on the top metal layer. The passivation layer 800 may be formed by etching through a photolithography process and includes a three-layer structure, namely, plasma enhanced oxide (PEOX), plasma enhanced silicon nitride (PESIN) and polyimide. The specific structure is as follows: Fig. 9 shown.

[0081] In the process of preparing the silicon carbide-based hybrid diode in the embodiment of the present invention, an ohmic contact groove 500 is etched in the first P-type doping region 410, and the ohmic metal 510 is filled in the ohmic contact groove 500, so that in the first P-type doping region 410, the P-type impurities that make ohmic contact with the ohmic metal 510 can be located on the silicon surfaces of the two side walls and the bottom of the first P-type doping region 410, so that the ohmic contact area of ​​the P-type impurities in the first P-type doping region 410 can be greatly increased, and the increase in the contact area means that the current can be more evenly distributed over a larger area, which reduces the local current density and reduces the risk of heat accumulation and electromigration, thereby improving the thermal stability and reliability of the device; and due to the increase in the contact area, the device can withstand a larger forward transient current without overheating or damage, which is particularly important for applications that need to handle large currents; in addition, the reverse withstand voltage can be improved, because the reverse ohmic metal is used as a field plate, which can improve the electric field distribution and increase the reverse breakdown voltage of the device, which means that under reverse bias conditions, the device can withstand a higher voltage without being broken down. In summary, the present invention can solve a series of problems caused by the small ohmic contact area of ​​the traditional MPS in the prior art.

[0082] In an optional implementation, after etching the ohmic contact trench 500 in the first active region by a photolithography process and before filling the ohmic metal 510 in the ohmic contact trench 500, the method further includes:

[0083] P-type impurities are injected into the bottom of the ohmic contact trench 500 to form a P-type impurity barrier 900 at the bottom of the ohmic contact trench 500. Fig.10 shown.

[0084] It can be understood that forming the P-type impurity barrier 900 at the bottom of the ohmic contact trench 500 can effectively avoid the premature breakdown due to the electric field concentration in the ohmic trench.

[0085] It should be noted that when the P-type impurities are injected into the bottom of the ohmic contact trench 500 , the impurity injection angle may be inclined with respect to the sidewall so that the P-type impurities can be injected into the bottom of the ohmic contact trench 500 .

[0086] As a specific example, before injecting P-type impurities into the bottom of the ohmic contact trench 500, the shielding layer used in the previous photolithography step can be removed, LPTEOS is retained, and the energy of the injection along the sidewall is 35-40kev and the dose is 5-6E15 / cm 3 of aluminum.

[0087] It can be understood that the P-type impurity barrier 900 is formed at the bottom of the ohmic contact trench 500, which can make the silicon carbide-based hybrid diode have a higher reverse breakdown voltage, a lower forward conduction voltage, and a higher current density.

[0088] In an optional implementation, the sputtering of Schottky metal 600 on the surface of the second active region in the cell region includes:

[0089] Etching a Schottky trench 610 on the surface of the second active region;

[0090] A Schottky metal 600 is sputtered in the Schottky trench 610 , and the Schottky metal 600 is alloyed with silicon carbide to form a Schottky barrier.

[0091] It should be noted that the second active region and the first active region are different active regions in the cell region.

[0092] In this implementation, the Schottky trench 610 may be etched on the surface of the second active region by a photolithography process, and the specific photolithography process may be set according to specific needs of the application.

[0093] As a specific example, Fig.11As shown, LPTEOS620 (or silicon dioxide) can be deposited on the top surface of the epitaxial layer first, and then a pattern is formed by photolithography, and then LPTEOS620 is etched as a shielding layer, and finally the Schottky trench 610 is etched. The depth of the etched Schottky trench 610 can be 0.4-0.6um, and the width can be 2-4um.

[0094] It can be understood that by etching the Schottky groove 610 and sputtering the Schottky metal 600 in the Schottky groove 610, since the area of ​​the Schottky groove 610 that can sputter the Schottky metal 600 includes the side area and the bottom area in the Schottky groove 610, the area of ​​the Schottky metal 600 finally sputtered in the silicon carbide-based hybrid diode finally obtained by this implementation is larger than the area of ​​the Schottky metal 600 directly sputtered on the surface of the device in the traditional silicon carbide-based hybrid diode, the forward voltage drop of the same area will be lower, and the reverse recovery time will be shorter. When the forward voltage drop is the same, the die area should be smaller.

[0095] In an optional implementation, after the N-type silicon carbide epitaxial layer 200 is grown on the front surface of the N-type silicon carbide substrate 100 and before the ohmic contact trench 610 is formed in the first active region by etching through a photolithography process, the method further includes:

[0096] P-type impurities are injected into the terminal region of the cell region of the N-type silicon carbide epitaxial layer 200 to generate a second P-type doped region 420. The specific structure is as follows Fig.12 shown.

[0097] It should be noted that the method of injecting P-type impurities into the terminal region of the cell region of the N-type silicon carbide epitaxial layer 200 to generate the second P-type doped region 420 may be any achievable method.

[0098] Optionally, in the present implementation, before injecting P-type impurities into the terminal region of the cell region of the N-type silicon carbide epitaxial layer 200, a first region into which P-type impurities need to be injected can be determined by a photolithography process, and the first region here can be obtained by the same photolithography process as the injection region (second region) for obtaining the first P-type doped region 410, that is, the first region and the second region can be ultimately etched simultaneously by one photolithography process, and further, P-type impurities can be simultaneously injected into the first region and the second region to obtain the second P-type doped region 420 and the first P-type doped region 410.

[0099] As a specific example, the number of second P-type doping regions 420 formed can be multiple, and the width and spacing of the multiple second P-type doping regions 420 can be determined according to the specific needs of the application. For example, the width of the second P-type doping region 420 can be 1-3um and the spacing can be 1-1.5um.

[0100] It is understandable that the electric field curvature at the edge of the terminal will become larger. By providing a second P-type doping region 420 in the terminal region, the electric field curvature can be reduced and the reverse withstand voltage of the product can be improved.

[0101] In an optional implementation, the doping concentration of the P-type impurity barrier is greater than the doping concentration of the first P-type doping region 410 .

[0102] It can be understood that when the doping concentration of the P-type impurity barrier 900 is greater than the doping concentration of the first P-type doping region 410 , it can be ensured that the curvature of the terminal edge electric field will decrease.

[0103] In an optional implementation, the width of the first P-type doping region 410 is greater than the width of the second P-type doping region 420 .

[0104] In an optional implementation, the P-type impurity is aluminum.

[0105] It should be noted that since nickel will melt when injected at high temperature, in this implementation, it is the best choice to inject aluminum into the N-type silicon carbide substrate 100 .

[0106] In an optional implementation, etching the ohmic contact groove 500 in the first active region by a photolithography process includes:

[0107] Depositing LPTEOS as a barrier layer 511 on the surface of the cell region;

[0108] Sputtering nickel on the LPTEOS as an etching blocking layer 512;

[0109] Etch the shielding layer 512 and the blocking layer 511 by a photolithography process, and remove the photoresist after the etching is completed;

[0110] The exposed surface of the cell region is etched to form an ohmic contact trench 500 .

[0111] Specific structure such as Figure 4 shown.

[0112] Optionally, the exposed surface of the cell region may be etched by dry etching, so that when LPTEOS is used as the barrier layer 511, dry etching can ensure a better morphology.

[0113] As a specific example, in the present implementation, the thickness of the blocking layer 511 may be 4500-5500A, the thickness of the shielding layer 512 may be 800-1200A, the depth of the ohmic contact groove 500 may be 0.8-1.2um, and the width may be 0.8-1.2um.

[0114] It can be understood that sputtering nickel to form the etching blocking layer 412 can make the selectivity of silicon carbide higher during etching.

[0115] In an optional implementation, the Schottky metal 600 is titanium.

[0116] Understandably, titanium bonds better with silicon carbide.

[0117] like Fig.13 FIG. 1 is a schematic diagram of a structure of a silicon carbide-based hybrid diode provided by an embodiment of the present invention, comprising:

[0118] N-type silicon carbide substrate 100;

[0119] An ohmic metal layer 300 is formed on the back side of the N-type silicon carbide substrate 100;

[0120] An N-type silicon carbide epitaxial layer 200 is grown on the front surface of the N-type silicon carbide substrate 100, and an ohmic contact groove 500 is etched in the first active region of the cell region, and a Schottky groove 610 is etched in the second active region of the cell region;

[0121] Schottky metal 600 is formed on the surface of the Schottky trench 610;

[0122] Ohmic metal 510, filled in the ohmic contact groove 500;

[0123] A first P-type doped region 410 is located in a first active region of a cell region of the N-type silicon carbide epitaxial layer 200 , and the ohmic contact trench 500 is located in the first P-type doped region 410 ;

[0124] A P-type impurity barrier 900 is formed at the bottom of the ohmic contact trench 500 , and the doping concentration of the P-type impurity barrier 900 is greater than the doping concentration of the first P-type doping region 410 ;

[0125] The second P-type doped region 420 is located at the terminal region of the N-type silicon carbide epitaxial layer 200 .

[0126] In the silicon carbide-based hybrid diode of the embodiment of the present invention, an ohmic contact groove 500 is etched in the first P-type doping region 410, and an ohmic metal 510 is filled in the ohmic contact groove 500, so that in the first P-type doping region 410, the P-type impurities that make ohmic contact with the ohmic metal 510 can be located on the two side walls and the bottom silicon surface in the first P-type doping region 410, so that the ohmic contact area of ​​the P-type impurities in the first P-type doping region 410 can be greatly increased, and the increase in the contact area means that the current can be more evenly distributed over a larger area, which reduces the local current density and reduces the risk of heat accumulation and electromigration, thereby improving the thermal stability and reliability of the device; and due to the increase in the contact area, the device can withstand a larger forward transient current without overheating or damage, which is particularly important for applications that need to handle large currents; in addition, the reverse withstand voltage can be improved, because the reverse ohmic metal is used as a field plate, which can improve the electric field distribution and increase the reverse breakdown voltage of the device, which means that under reverse bias conditions, the device can withstand a higher voltage without being broken down. In summary, the present invention can solve a series of problems caused by the small ohmic contact area of ​​the traditional MPS in the prior art.

[0127] The technical solution provided by the present application is introduced in detail above. The principles and implementation methods of the present application are explained by using specific examples in the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

[0128] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A method for preparing a silicon carbide-based hybrid diode, characterized in that: include: Obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating an ohmic metal layer on the back surface of the N-type silicon carbide substrate; Injecting P-type impurities into a first active region of a cell region of the N-type silicon carbide epitaxial layer to generate a first P-type doped region; Etching an ohmic contact groove in the first active region by a photolithography process, wherein the ohmic contact groove is located in the first P-type doped region; Filling the ohmic contact groove with ohmic metal; A Schottky metal is sputtered on the surface of the second active region in the cell region.

2. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: After etching the ohmic contact trench in the first active region by a photolithography process and before filling the ohmic contact trench with an ohmic metal, the method further includes: P-type impurities are implanted into the bottom of the ohmic contact trench to form a P-type impurity barrier at the bottom of the ohmic contact trench.

3. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: The sputtering of Schottky metal on the surface of the second active region in the cell region comprises: Etching a Schottky trench on the surface of the second active region; A Schottky metal is sputtered in the Schottky trench, and the Schottky metal is alloyed with silicon carbide to form a Schottky barrier.

4. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: After growing an N-type epitaxial layer on the front surface of the N-type silicon carbide substrate and before etching to form an ohmic contact trench in the first active region by a photolithography process, the method further includes: P-type impurities are implanted into the terminal region of the cell region of the N-type silicon carbide epitaxial layer to generate a second P-type doped region.

5. The method for preparing a silicon carbide-based hybrid diode according to claim 2, characterized in that: The doping concentration of the P-type impurity barrier is greater than the doping concentration of the first P-type doping region.

6. The method for preparing a silicon carbide-based hybrid diode according to claim 4, characterized in that: The width of the first P-type doping region is greater than the width of the second P-type doping region.

7. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: The P-type impurity is aluminum.

8. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: The etching to form an ohmic contact groove in the first active region by a photolithography process comprises: Depositing LPTEOS as a barrier layer on the surface of the cell region; Sputtering nickel on the LPTEOS as an etching shielding layer; Etching the shielding layer and the blocking layer by a photolithography process, and removing the photoresist after the etching is completed; The exposed surface of the cell region is etched to form an ohmic contact groove.

9. The method for preparing a silicon carbide-based hybrid diode according to claim 1, characterized in that: The Schottky metal is titanium.

10. A silicon carbide-based hybrid diode, characterized in that: include: N-type silicon carbide substrate; An ohmic metal layer is formed on the back side of the N-type silicon carbide substrate; An N-type silicon carbide epitaxial layer is grown on the front surface of the N-type silicon carbide substrate, and an ohmic contact groove is etched in the first active region of the cell region, and a Schottky groove is etched in the second active region of the cell region; A Schottky metal is formed on the surface of the Schottky trench; Ohmic metal, filled in the ohmic contact groove; A first P-type doped region is located in a first active region of a cell region of the N-type silicon carbide epitaxial layer, and the ohmic contact trench is located in the first P-type doped region; A P-type impurity barrier is formed at the bottom of the ohmic contact trench, and the doping concentration of the P-type impurity barrier is greater than the doping concentration of the first P-type doping region; The second P-type doped region is located in the terminal region of the N-type silicon carbide epitaxial layer.

Citation Information

Cited By

  • Semiconductor device, preparation method of semiconductor device and chip

    CN119947139A