Positive electrode capable of limiting lattice oxygen escape and preparation method and application thereof

By adding lattice oxygen inhibitors to the positive electrode of the secondary battery, the release of reactive oxygen is suppressed, and the problem of thermal runaway for nickel-rich lithium-ion batteries is solved, and the safety and circulation performance of the battery are improved.

CN119050267AActive Publication Date: 2024-11-29HUAZHONG UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411086486.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-29
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively suppress the thermal runaway of nickel-rich lithium-ion batteries, mainly because reactive oxygen species are released too quickly at high temperatures, resulting in rapid battery temperature rise, which makes it difficult for external auxiliary systems to control.

Method used

Add lattice oxygen inhibitors, such as phytate, α-gluheptanonate, etc. to the positive electrode of the secondary battery, and combine conductive agents and adhesives to form a glue solution. The lattice oxygen escape can be prepared by baking. , thereby inhibiting the release and reaction of reactive oxygen species.

Benefits of technology

It effectively delays the occurrence of thermal runaway, improves battery safety, reduces the risk of thermal runaway, and significantly improves the cycle performance and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050267A_ABST
    Figure CN119050267A_ABST
Patent Text Reader

Abstract

The invention discloses a positive electrode capable of limiting lattice oxygen escape and a preparation method and application thereof. The specific method is that a lattice oxygen inhibitor is added into the positive electrode of a secondary battery. The lattice oxygen inhibitor not only can serve as the role of a physical passivation film to constrain particle volume change and prevent direct contact of an electrode / electrolyte, but also can serve as the role of an electron library to inhibit loss of interface lattice oxygen and transformation of harmful interface phase transformation in an interface charge compensation mode. The lattice oxygen release of nickel-rich layered oxide, lithium cobalt oxide, lithium manganate, lithium-rich manganese-based and sodium-based layered oxide positive electrode materials at high temperature is greatly inhibited through the two effects, and the chemical crosstalk reaction between active oxygen and an organic solvent and between the active oxygen and a lithiated negative electrode is weakened. Therefore, the heat accumulation of the thermal runaway trigger point can be effectively restrained, the thermal runaway of the battery is delayed or avoided, and the safety of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a secondary battery positive electrode capable of limiting lattice oxygen escape, and a preparation method and application thereof. Background Art

[0002] With the rapid development of electric vehicles and smart grids, the demand for high energy density lithium-ion batteries (LIBs) in these emerging fields has increased dramatically. High-capacity, low-cost nickel-rich layered oxides LiNixCoyMnzO2 (NCM) are considered to be one of the most promising candidates for high energy density lithium-ion batteries. Unfortunately, the increase in nickel content will correspondingly increase the possibility of thermal runaway (TR). Ni-rich NCMs batteries are prone to thermal runaway, resulting in a large amount of energy release, which increases the battery temperature to about 1000°C. In this case, the external auxiliary battery management system (BMS) or fire extinguishing system is basically ineffective. The violent redox reaction between the strongly reducing lithiated graphite (LiCx) and the highly oxidizing nickel-rich dilithiated NCM is the key catalyst to trigger TR. Once the temperature exceeds the TR trigger point, many unique side reactions will be rapidly and simultaneously initiated within seconds. At the same time, the heating rate of the battery will increase by several orders of magnitude and instantly reach the catastrophic temperature during TR. Therefore, suppressing the characteristic conversion flow between the cathode and anode at the TR trigger point is the key to suppressing TR.

[0003] As the number of cycles increases and the temperature rises, the de-lithiated nickel-rich layered oxide is very likely to undergo a structural phase change. During this process, the lattice oxygen in the bulk phase of the material will break free and form reactive oxygen species (ROS, O*). Studies have shown that in the absence of an internal short circuit, the crosstalk reaction caused by reactive oxygen (O*) is the direct cause of thermal runaway in ternary lithium-ion batteries. In addition, the thermal runaway trigger temperature will be lower as the nickel content increases. This is because as the nickel content increases, the degree of hybridization of the Ni-O bond increases, and under high temperature conditions, it will further promote the participation of oxygen anions in charge compensation within the Ni-O bond, thereby promoting the release of O*. Therefore, alleviating the thermal runaway of ternary lithium-ion batteries can start from weakening the participation of oxygen anions in charge compensation within the Ni-O bond, limiting the release of reactive oxygen, and achieving the purpose of suppressing thermal runaway. The tricky thing is that there is still no effective strategy to solve the TR problem caused by O*. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a positive electrode that can limit the escape of lattice oxygen and improve the safety of secondary batteries. It can stabilize the lattice oxygen in the bulk phase of the material to limit the release of active oxygen from the positive electrode material at high temperature, inhibit the continuous reaction between active oxygen and the electrolyte and the lithiated graphite negative electrode, and achieve the purpose of delaying thermal runaway and improving battery safety.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A positive electrode capable of limiting lattice oxygen escape, the positive electrode comprising an active material, a conductive agent, a binder, and a lattice oxygen inhibitor;

[0007] The lattice oxygen inhibitor is one or more of phytate, α-glucoheptonate, tert-butyl ester compound, tetrasodium iminodisuccinate, sodium hexametaphosphate, sodium tripolyphosphate, oxalate, citric acid or citrate, aminocarboxylic acid compounds, organic polyphosphonic acid, phosphates, and thiol (-SH) containing compounds.

[0008] Furthermore, the active material accounts for 80-95% by weight in the positive electrode; the conductive agent accounts for 1-10% by weight in the positive electrode; the binder accounts for 1-10% by weight in the positive electrode; and the lattice oxygen inhibitor accounts for 0.1-5% by weight in the positive electrode.

[0009] Furthermore, the active material is nickel-rich layered oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium-rich manganese-based oxide and sodium-based layered oxide.

[0010] Furthermore, the phytate structure is shown in Formula I and Formula II:

[0011]

[0012] Among them, R 1 At least one of monovalent metal ions such as lithium ion, sodium ion, potassium ion, etc.;

[0013]

[0014] Among them, R 2 At least one of divalent metal ions such as barium ion, copper ion, calcium ion, zinc ion, cobalt ion, magnesium ion, etc.;

[0015] The structure of the aminocarboxylic acid compound is shown in Formula III:

[0016]

[0017] Among them, R 3 At least one of diacetylamino, acetyl, ethylenediaminetriacetyl, hydroxyl, ethyl, phenyl, vinyl, acetoxy, acetoxyethyl, 3-acryloyl, 3-methacryloyl, and N,N-dipropyl;

[0018] The structure of the thiol compound is shown in Formula IV:

[0019]

[0020] Among them, R 4 At least one of isooctyl acetate, propionate, 2-butanone, ethylamine, ethanol, butyrate, acetaldehyde, succinate, 1,3,4-thiadiazolyl, acetate, thiol, naphthyl, methyl acetate, acetylnaphthylamine, ethyl acetate, benzyl acetate, sodium pyruvate, thiadiazolyl, and benzoate;

[0021] In some specific embodiments, preferably, the phytate is at least one of lithium phytate, sodium phytate, potassium phytate, barium phytate, copper phytate, calcium phytate, zinc phytate, cobalt phytate, and magnesium phytate;

[0022] The aminocarboxylic acid compound is at least one of ethylenediaminetetraacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, N-hydroxyethylethylaminetriacetic acid ethylene glycol-bis-(B-aminoethyl ether)-N,N-tetraacetic acid;

[0023] The thiol compound is at least one of isooctyl thioglycolate, mercaptopropionic acid, 3-mercapto-2-butanone, β-mercaptoethylamine, mercaptoethanol, mercaptobutyric acid, mercaptoacetaldehyde, strontium thioglycolate, mercaptosuccinic acid, mercaptothiadiazole, magnesium thioglycolate, potassium thioglycolate, dimercaptomethane, 2-mercaptonaphthalene, methyl thioglycolate, mercaptoacetamide, benzyl thioglycolate, and 4-mercaptobenzyl.

[0024] Furthermore, the chemical formula of the nickel-rich layered oxide is LiNi x Co y Mn z O 2 (x+y+z=1);

[0025] The chemical formula of the lithium-rich manganese-based oxide is aLi 2 MnO 3 (1-a) LiMO 2 (M=Ni, Co, Mn);

[0026] The chemical formula of the sodium-based layered oxide is Na b MO 2 , (M represents transition metals such as nickel, cobalt, iron, and manganese), the value of b corresponds to the valence state of M.

[0027] Furthermore, the conductive agent is at least one of carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene.

[0028] Furthermore, the binder is at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene rubber, and sodium alginate.

[0029] In some specific embodiments, preferably, the active material is Li[Ni 0.8 Co0.1 Mn 0.1 ]O 2 The conductive agent is conductive carbon black, the adhesive is polyvinylidene fluoride, and the lattice oxygen inhibitor is sodium phytate, and they are mixed in a mass ratio of 80:x:10:y, where x+y=10.

[0030] A method for preparing the above-mentioned positive electrode capable of limiting lattice oxygen escape comprises the following steps:

[0031] The binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the glue solution in sequence and stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector with the positive electrode slurry scraped on it is baked to remove the N-methylpyrrolidone, thereby obtaining the positive electrode capable of limiting the escape of lattice oxygen.

[0032] A secondary battery comprises the secondary battery positive electrode for limiting lattice oxygen escape as mentioned above.

[0033] Furthermore, the secondary battery is a lithium ion battery, a lithium metal battery, a sodium ion battery or a sodium metal battery.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention discloses a positive electrode capable of limiting the escape of lattice oxygen, a preparation method thereof, and an application thereof in improving the safety of a secondary battery. The specific method is to add a lattice oxygen inhibitor to the positive electrode in the secondary battery. The lattice oxygen inhibitor can not only act as a "physical passivation film" to constrain the volume change of particles and prevent direct contact between electrodes and electrolytes, but also act as an "electron reservoir" to inhibit the loss of interfacial lattice oxygen and the conversion of harmful interfacial phase transitions by means of interfacial charge compensation. These two aspects greatly inhibit the release of lattice oxygen at high temperatures of nickel-rich layered oxides, lithium cobalt oxide, lithium manganese oxide, lithium-rich manganese-based and sodium-based layered oxide positive electrode materials, and weaken the chemical crosstalk reaction between active oxygen and organic solvents and lithiated negative electrodes. More importantly, since the lattice oxygen inhibitor can passivate the positive electrode material, delay the phase change oxygen evolution process of the de-lithium positive electrode or the de-sodium positive electrode at high temperature, the purpose of delaying the participation of active oxygen in the crosstalk reaction is achieved. Therefore, the heat accumulation at the thermal runaway trigger point can be effectively curbed, delaying or avoiding the occurrence of battery thermal runaway, and improving the safety of the battery.

[0036] The positive electrode and the electrolyte prepared by the present invention have a heat release rate between -120 J / g and -250 J / g, have a higher initial heat release temperature and a lower reaction heat release rate, can delay or even block the thermal runaway of the battery, and reduce the risk of thermal runaway of the battery; assembling the electrolyte prepared by the present invention into a soft-pack battery can significantly increase the trigger temperature of thermal runaway and reduce the maximum temperature during thermal runaway.

[0037] The positive electrode of the present invention is used to prepare a full battery with excellent cycle performance.

[0038] The preparation method of the invention is simple, requiring only simple stirring, mixing and filtering, and the raw materials are conventionally readily available, with low cost, and is suitable for vigorous promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 DSC curves of the positive electrodes of Comparative Example 1, Example 5, Example 10 and Example 15 and conventional carbonate electrolytes;

[0040] Figure 2 DSC curves of the positive electrode and lithiated graphite of Comparative Example 1 and Example 15;

[0041] Figure 3 DSC curves of the positive electrode of Comparative Example 3 and Example 30 and conventional carbonate electrolyte;

[0042] Figure 4 The temperature-time curves of the full batteries of Comparative Example 1, Example 5 and Example 15 in the heating experiment are shown;

[0043] Figure 5 The cycle capacity diagram of the full battery equipped with the positive electrodes of Comparative Example 1 and Example 5;

[0044] Figure 6 The cycle capacity diagram of the full battery equipped with the positive electrodes of Comparative Example 2 and Example 15;

[0045] Figure 7 This is a cycle capacity diagram of a full battery equipped with the positive electrodes of Comparative Example 4 and Example 30. DETAILED DESCRIPTION

[0046] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand the present invention more clearly.

[0047] The specific raw materials not described in the present invention are all existing materials and can be directly purchased from the market. The present invention provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0048] The binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then a conductive agent, an active material, and a lattice oxygen inhibitor are added to the glue solution in sequence and stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector with the positive electrode slurry scraped on is baked to remove the N-methylpyrrolidone, thereby obtaining the positive electrode capable of limiting the escape of lattice oxygen;

[0049] The lattice oxygen inhibitor is one or more of phytate, α-glucoheptonate, tert-butyl ester compound, tetrasodium iminodisuccinate, sodium hexametaphosphate, sodium tripolyphosphate, oxalate, citric acid or citrate, aminocarboxylic acid compounds, organic polyphosphonic acid, phosphates, and thiol (-SH) containing compounds.

[0050] In some specific embodiments, the weight percentage of the active material in the positive electrode is 80-95%; the weight percentage of the conductive agent in the positive electrode is 1-10%; the weight percentage of the binder in the positive electrode is 1-10%; and the weight percentage of the lattice oxygen inhibitor in the positive electrode is 0.1-5%.

[0051] The active material is one of nickel-rich layered oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium-rich manganese-based oxide and sodium-based layered oxide.

[0052] The conductive agent is one of carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0053] The binder is one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene rubber and sodium alginate.

[0054] In some specific embodiments, the chemical formula of the nickel-rich layered oxide is LiNi x Co y Mn z O 2 , x+y+z=1;

[0055] The chemical formula of the lithium-rich manganese-based oxide is aLi 2 MnO 3 (1-a) LiMO 2 , wherein M is Ni, Co or Mn;

[0056] The chemical formula of the sodium-based layered oxide is Na b MO 2 (M represents transition metals such as nickel, cobalt, iron, and manganese), and the value of b corresponds to the valence state of M.

[0057] In some specific embodiments, the active material is Li[Ni 0.8 Co0.1 Mn 0.1 ]O 2 The conductive agent is conductive carbon black, the adhesive is polyvinylidene fluoride, and the lattice oxygen inhibitor is sodium phytate, and they are mixed in a mass ratio of 80:x:10:y, where x+y=10.

[0058] In some specific embodiments, the phytate structure is as shown in Formula I and Formula II:

[0059]

[0060] Among them, R 1 At least one of monovalent metal ions such as lithium ion, sodium ion, potassium ion, etc.;

[0061]

[0062] Among them, R 2 At least one of divalent metal ions such as barium ion, copper ion, calcium ion, zinc ion, cobalt ion, magnesium ion, etc.;

[0063] The structure of the aminocarboxylic acid compound is shown in Formula III:

[0064]

[0065] Among them, R 3 At least one of diacetylamino, acetyl, ethylenediaminetriacetyl, hydroxyl, ethyl, phenyl, vinyl, acetoxy, acetoxyethyl, 3-acryloyl, 3-methacryloyl, and N,N-dipropyl;

[0066] The structure of the thiol compound is shown in Formula IV:

[0067]

[0068] Among them, R 4 It is at least one of isooctyl acetate, propionate, 2-butanone, ethylamine, ethanol, butyrate, acetaldehyde, succinate, 1,3,4-thiadiazolyl, acetate, thiol, naphthyl, methyl acetate, acetylnaphthylamine, ethyl acetate, benzyl acetate, sodium pyruvate, thiadiazolyl, and benzoate.

[0069] More preferably, in some specific embodiments, the phytate is at least one of lithium phytate, sodium phytate, potassium phytate, barium phytate, copper phytate, calcium phytate, zinc phytate, cobalt phytate, and magnesium phytate;

[0070] The aminocarboxylic acid compound is at least one of ethylenediaminetetraacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, N-hydroxyethylethylaminetriacetic acid ethylene glycol-bis-(B-aminoethyl ether)-N,N-tetraacetic acid;

[0071] The thiol compound is at least one of isooctyl thioglycolate, mercaptopropionic acid, 3-mercapto-2-butanone, β-mercaptoethylamine, mercaptoethanol, mercaptobutyric acid, mercaptoacetaldehyde, strontium thioglycolate, mercaptosuccinic acid, mercaptothiadiazole, magnesium thioglycolate, potassium thioglycolate, dimercaptomethane, 2-mercaptonaphthalene, methyl thioglycolate, mercaptoacetamide, benzyl thioglycolate, and 4-mercaptobenzyl.

[0072] Examples 1-5

[0073] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0074] The active material is Li[Ni 0.8 Co 0.1 Mn 0.1 ]O 2 (NCM811), the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, the lattice oxygen inhibitor is mercaptoacetyl naphthylamine, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 1 below.

[0075] Examples 6-10

[0076] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0077] The active material is Li[Ni 0.8 Co 0.1 Mn 0.1 ]O 2 (NCM811), the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, and the lattice oxygen inhibitor is nitrilotriacetic acid, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 1 below.

[0078] Examples 10-15

[0079] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0080] The active material is Li[Ni 0.8 Co 0.1 Mn 0.1 ]O 2 (NCM811), the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, the lattice oxygen inhibitor is sodium phytate, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 1 below.

[0081] Table 1 Details of active materials and lattice oxygen inhibitor content in lithium battery positive electrode

[0082] Serial number Active material content (%) Lattice oxygen inhibitor content (%) Example 1 80 0.1 Example 2 80 0.5 Example 3 80 1 Example 4 80 3 Example 5 80 5 Example 6 80 0.1 Example 7 80 0.5 Example 8 80 1 Example 9 80 3 Example 10 80 5 Embodiment 11 80 0.1 Example 12 80 0.5 Example 13 80 1 Embodiment 14 80 3 Embodiment 15 80 5

[0083] Examples 16-20

[0084] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0085] The active material is selected as NaNi 0.4 Fe 0.2 Mn 0.4 O 2 , the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, the lattice oxygen inhibitor is diethylenetriaminepentaacetic acid, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove the N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 2 below.

[0086] Examples 21-25

[0087] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0088] The active material is selected as NaNi 0.4 Fe0.2 Mn 0.4 O 2 , the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, the lattice oxygen inhibitor is 2-mercaptonaphthalene, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove the N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 2 below.

[0089] Examples 26-30

[0090] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0091] The active material is selected as NaNi 0.4 Fe 0.2 Mn 0.4 O 2 , the conductive agent is conductive carbon black, the binder is polyvinylidene fluoride, the lattice oxygen inhibitor is cobalt phytate, and the mass ratio is 80:x:1:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 2 below.

[0092] Table 2 Details of active materials and lattice oxygen inhibitor content in sodium positive electrode

[0093]

[0094]

[0095] Embodiment 31

[0096] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0097] The active material is lithium manganese oxide, the conductive agent is conductive graphite, the binder is polytetrafluoroethylene, and the lattice oxygen inhibitor is barium phytate, and the mass ratio is 80:x:10:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 3 below.

[0098] Embodiment 32

[0099] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0100] The active material is lithium nickelate, the conductive agent is carbon fiber, the adhesive is sodium carboxymethyl cellulose, and the lattice oxygen inhibitor is β-mercaptoethylamine in a mass ratio of 80:x:1:y, x+y=10. First, the adhesive is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or carbon-coated aluminum foil current collector; finally, the current collector scraped with the positive electrode slurry is baked to remove N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 3 below.

[0101] Embodiment 33

[0102] This embodiment provides a method for preparing a positive electrode capable of limiting lattice oxygen escape, comprising the following steps:

[0103] The active material is lithium cobalt oxide, the conductive agent is carbon nanotubes, the adhesive is styrene-butadiene rubber, and the lattice oxygen inhibitor is tetrasodium iminodisuccinate in a mass ratio of 80:x:1:y, x+y=10. First, the binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, the active material, and the lattice oxygen inhibitor are added to the above glue solution in turn and stirred evenly to obtain a positive electrode slurry; the above positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector with the positive electrode slurry is baked to remove the N-methylpyrrolidone, and the positive electrode capable of limiting the escape of lattice oxygen is obtained. The specific material ratios in the positive electrode are shown in Table 3 below.

[0104] Table 3 Details of active materials and lattice oxygen inhibitor content in sodium positive electrode

[0105] Serial number Active material content (%) Lattice oxygen inhibitor content (%) Embodiment 31 80 1.5 Embodiment 32 80 2 Embodiment 33 80 4

[0106] Comparative Example 1

[0107] This comparative example provides a method for preparing a positive electrode capable of limiting the escape of lattice oxygen, and its principles and steps are basically the same as those of the experiment No. 1 in Example 1, except that the lattice oxygen inhibitor is removed.

[0108] Comparative Example 2

[0109] This comparative example provides a method for preparing a positive electrode capable of limiting the escape of lattice oxygen, and its principles and steps are basically the same as those of the experiment No. 1 in Example 1, except that the content of active material is 80% and the content of lattice oxygen inhibitor is 6%.

[0110] Comparative Example 3

[0111] This comparative example provides a method for preparing a positive electrode that can limit the escape of lattice oxygen. Its principles and steps are basically the same as those of experiment No. 1 in Example 16, except that the lattice oxygen inhibitor is removed.

[0112] Comparative Example 4

[0113] This comparative example provides a method for preparing a positive electrode that can limit the escape of lattice oxygen. Its principles and steps are basically the same as those of experiment No. 1 in Example 16, except that the active material content is 80% and the lattice oxygen inhibitor content is 6%.

[0114] Performance Verification

[0115] In order to further verify the performance of the positive electrode prepared above, the following performance tests were performed on it:

[0116] (1) The positive electrode and electrolyte prepared in Examples 1-15 and Comparative Examples 1 and 2 were assembled into a graphite|NCM811 full battery, and the half-cell was cycled for 5 cycles at a current density of 0.1C to form a stable CEI film. After the cycle was completed, the battery was disassembled in a glove box filled with argon, and the charged positive electrode plates of each embodiment obtained by disassembly were cleaned with dimethyl carbonate to remove the residual lithium salt and solvent on the surface of the plate, and then placed in a glove box filled with argon to dry. About 4 mg of charged positive electrode powder was scraped from the dried plate and placed in an aluminum crucible for a differential scanning calorimeter (DSC 4000, PerkinElmer), and about 5 mg of electrolyte was added dropwise. DSC test was performed to detect the heat released by the reaction between the charged positive electrode powder and the electrolyte. The heat release test results of the positive electrodes and electrolytes prepared in Examples 1-15 and Comparative Examples 1 and 2 are shown in Table 4; the DSC curves of the charged positive electrode powders and electrolytes of Comparative Example 1, Example 5, Example 10, and Example 15 are shown in Table 4. Figure 1 shown.

[0117] Table 4 Test results of heat release between the positive electrode and the electrolyte prepared in Examples 1-15 and Comparative Examples 1 and 2

[0118]

[0119]

[0120] Depend on Figure 1 It can be seen that the reaction heat released by the electrolyte of comparative example 1 and the charged conventional lithium battery positive electrode is as high as -319.8 J / g, while after adding the lattice oxygen inhibitor, the reaction heat released by Examples 5, 10 and 15 is reduced to -245.3, -200.2 and -121.6 J / g, respectively.

[0121] (2) The lithiated graphite electrode pieces and the charged positive electrode obtained by disassembling Comparative Example 1 and Example 15 were placed in two aluminum crucibles of different sizes, respectively. The charged positive electrode was placed in a small crucible, and the lithiated graphite obtained by Comparative Example 1 and Example 15 were placed in a large crucible. The bottom of the small crucible containing the charged positive electrode was pierced with a large number of small holes in advance so that the generated active oxygen could smoothly reach the lithiated graphite. Figure 2 The DSC curves of the charged positive electrodes of Comparative Example 1 and Example 15 are shown respectively.

[0122] Depend on Figure 2 It can be seen that the use of Example 15 containing an active oxygen inhibitor can significantly reduce the heat released by active oxygen and lithiated graphite.

[0123] (3) The positive electrodes and electrolytes prepared in Examples 16-30 and Comparative Examples 3 and 4 were assembled into hard carbon

[0124] ∣NaNi 0.4 Fe 0.2 Mn 0.4 O 2 For a full cell, the half cell is cycled 5 times at a current density of 0.1C to form a stable CEI film. After the cycle is completed, the battery is disassembled in a glove box filled with argon, and the charged positive electrode plates of each embodiment obtained by disassembly are cleaned with dimethyl carbonate to remove the residual sodium salt and solvent on the surface of the plate, and then placed in a glove box filled with argon to dry. Scrape about 4 mg of charged positive electrode powder from the dried plate and place it in an aluminum crucible for DSC, add about 5 mg of electrolyte, and perform DSC test to detect the heat released by the reaction between the charged positive electrode powder and the electrolyte of each embodiment. The heat release test results of the positive electrode and the electrolyte prepared in Examples 16-30 and Comparative Examples 3 and 4 are shown in Table 5; the DSC curves of the charged positive electrode powder and the electrolyte of Comparative Example 3 and Example 30 are shown in Table 5. Figure 3 shown.

[0125] Table 5 Test results of heat release between the positive electrode and the electrolyte prepared in Examples 16-30, Comparative Examples 3 and 4

[0126]

[0127]

[0128] Depend on Figure 3 It can be seen that the reaction heat released by the electrolyte of comparative example 3 and the charged conventional sodium positive electrode is as high as -577.2 J / g, while after adding the lattice oxygen inhibitor, the reaction heat released by Example 30 is reduced to -302.2 J / g.

[0129] (4) A heating experiment was conducted using the soft battery packs containing the positive electrodes prepared in Example 5, Example 15, and Comparative Example 1 to obtain the temperature-time relationship. The results are shown in FIG. Figure 4 .

[0130] Depend on Figure 4 It can be seen that the trigger temperature of thermal runaway in comparative example 1 is 154.1°C, and the trigger temperatures of thermal runaway in examples 5 and 15 are 196.0°C and 254.0°C, respectively; the maximum temperature during thermal runaway in comparative example 1 is 1191.9°C, and the maximum temperatures during thermal runaway in examples 5 and 15 are 895.8°C and 729.2°C, respectively. The use of soft-pack batteries containing electrolytes in examples 5 and 15 can significantly increase the trigger temperature of thermal runaway and reduce the maximum temperature during thermal runaway.

[0131] (5) The positive electrodes prepared in Examples 1-15 and Comparative Examples 1 and 2 were assembled with electrolytes, negative electrodes and separators into NCM811|graphite full batteries. The first cycle discharge specific capacity (mAh / g) and the capacity retention rate after 100 cycles are shown in Table 6. Figure 5 , Figure 6 They are cycle performance diagrams obtained from full battery tests containing positive electrodes of Comparative Example 1, Example 5, Comparative Example 2, and Example 15, respectively.

[0132] Table 6 Full battery discharge capacity and capacity retention data of positive electrodes prepared in Examples 1-15, Comparative Examples 1 and 2

[0133]

[0134] Comprehensive Table 6, Figure 5 , 6 It can be seen that the electrochemical performance of the positive electrode provided by the embodiment of the present invention is better than that of comparative examples 1 and 2, which indicates that the addition of the active oxygen inhibitor in the embodiment of the present invention does not have a negative impact on the electrochemical performance. However, once the amount of active oxygen inhibitor added exceeds the weight percentage provided by the present invention, it will lead to poor cycle performance.

[0135] (7) The lithium battery positive electrode prepared in Examples 16-30, Comparative Examples 3 and 4 was assembled with the electrolyte, negative electrode and separator into a NaNi 0.4 Fe 0.2 Mn 0.4 O2 | Hard carbon full battery, the first cycle discharge specific capacity (mAh / g) and the capacity retention rate after 300 cycles are shown in Table 7; Figure 7 This is a cycle performance diagram obtained from a full battery test containing the positive electrodes of Comparative Example 4 and Example 16.

[0136] Table 7 Discharge capacity and capacity retention rate data of full batteries containing positive electrodes prepared in Examples 16-30, Comparative Examples 3 and 4

[0137]

[0138]

[0139] Comprehensive Table 7, Figure 7 It can be seen that the electrochemical performance of the sodium positive electrode provided by the embodiment of the present invention is better than that of comparative examples 3 and 4, which shows that the addition of the active oxygen inhibitor in the embodiment of the present invention does not have a negative impact on the electrochemical performance. However, once the amount of active oxygen inhibitor added exceeds the weight percentage provided by the present invention, it will lead to poor cycle performance.

[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A positive electrode capable of limiting the escape of lattice oxygen, characterized in that: The positive electrode comprises an active material, a conductive agent, a binder, and a lattice oxygen inhibitor; The lattice oxygen inhibitor is one or more of phytate, α-glucoheptonate, tert-butyl ester compound, tetrasodium iminodisuccinate, sodium hexametaphosphate, sodium tripolyphosphate, oxalate, citric acid, citrate, aminocarboxylic acid compounds, organic polyphosphonic acid, phosphates, and thiol-containing compounds.

2. A positive electrode capable of limiting lattice oxygen escape according to claim 1, characterized in that: The active material is a nickel-rich layered oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium-rich manganese-based oxide or sodium-based layered oxide; The active material accounts for 80-95% by weight in the positive electrode; the conductive agent accounts for 1-10% by weight in the positive electrode; the adhesive accounts for 1-10% by weight in the positive electrode; and the lattice oxygen inhibitor accounts for 0.1-5% by weight in the positive electrode.

3. A positive electrode capable of limiting lattice oxygen escape according to claim 1, characterized in that: The phytate structure is shown in Formula I or Formula II: Wherein, R1 is at least one of lithium ion, sodium ion and potassium ion; Wherein, R2 is at least one of barium ion, copper ion, calcium ion, zinc ion, cobalt ion and magnesium ion; The structure of the aminocarboxylic acid compound is shown in Formula III: Wherein, R3 is at least one of diacetylamino, acetyl, ethylenediaminetriacetyl, hydroxyl, ethyl, phenyl, vinyl, acetoxy, acetoxyethyl, 3-acryloyl, 3-methacryloyl, and N,N-dipropyl; The structure of the thiol compound is shown in Formula IV: HS-R4 Formula IV Among them, R4 is at least one of isooctyl acetate, propionate, 2-butanone, ethylamine, ethanol, butyrate, acetaldehyde, succinate, 1,3,4-thiadiazolyl, acetate, thiol, naphthyl, methyl acetate, acetylnaphthylamine, ethyl acetate, benzyl acetate, sodium pyruvate, thiadiazolyl, and benzoate.

4. A positive electrode capable of limiting lattice oxygen escape according to claim 1, characterized in that: The phytate is at least one of lithium phytate, sodium phytate, potassium phytate, barium phytate, copper phytate, calcium phytate, zinc phytate, cobalt phytate, and magnesium phytate; The aminocarboxylic acid compound is at least one of ethylenediaminetetraacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, N-hydroxyethylethylaminetriacetic acid ethylene glycol-bis-(B-aminoethyl ether)-N,N-tetraacetic acid; The thiol compound is at least one of isooctyl thioglycolate, mercaptopropionic acid, 3-mercapto-2-butanone, β-mercaptoethylamine, mercaptoethanol, mercaptobutyric acid, mercaptoacetaldehyde, strontium thioglycolate, mercaptosuccinic acid, mercaptothiadiazole, magnesium thioglycolate, potassium thioglycolate, dimercaptomethane, 2-mercaptonaphthalene, methyl thioglycolate, mercaptoacetylamine, benzyl thioglycolate, and 4-mercaptotoluene.

5. A positive electrode capable of limiting lattice oxygen escape according to claim 2, characterized in that: The chemical formula of the nickel-rich layered oxide is LiNi x Co y Mn z O2, x+y+z=1; The chemical formula of the lithium-rich manganese-based oxide is aLi2MnO3·(1-a)LiMO2, wherein M is Ni, Co or Mn; The chemical formula of the sodium-based layered oxide is Na b MO2, M is nickel, cobalt, iron or manganese, and the value of b is consistent with the valence state of M.

6. A positive electrode capable of limiting lattice oxygen escape according to claim 1, characterized in that: The conductive agent is at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene; the binder is at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene rubber, and sodium alginate.

7. A positive electrode capable of limiting lattice oxygen escape according to any one of claims 1 to 6, characterized in that: The active material is Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2, the conductive agent is conductive carbon black, the adhesive is polyvinylidene fluoride, and the lattice oxygen inhibitor is sodium phytate, and they are mixed in a mass ratio of 80:x:10:y, x+y=10.

8. A method for preparing a positive electrode capable of limiting lattice oxygen escape as claimed in claim 7, characterized in that: The following steps are involved: The binder is dissolved in N-methylpyrrolidone and stirred until a clear glue solution is formed; then the conductive agent, active material, and lattice oxygen inhibitor are added to the glue solution in sequence and stirred evenly to obtain a positive electrode slurry; the positive electrode slurry is scraped onto an aluminum foil or a carbon-coated aluminum foil current collector; finally, the current collector with the positive electrode slurry scraped on it is baked to remove the N-methylpyrrolidone, thereby obtaining the positive electrode capable of limiting the escape of lattice oxygen.

9. A secondary battery, characterized in that: The secondary battery comprises the positive electrode capable of limiting lattice oxygen escape as claimed in claim 7, and the secondary battery is a lithium ion battery, a lithium metal battery, a sodium ion battery or a sodium metal battery.

10. Use of the positive electrode capable of limiting lattice oxygen escape as claimed in claim 7 in improving the safety of secondary batteries.

Citation Information

Patent Citations

  • Positive electrode lithium supplement agent and preparation method and application thereof

    CN115332520A

  • Monocrystal lithium-rich material, preparation method thereof and energy storage device

    CN116856058A

  • Alkaline storage battery

    JP2008257899A

  • Composite electrode of lithium ion secondary battery

    JP2014211978A