Preparation method of interface layer pre-lithiation dry method negative electrode of lithium-containing multi-element alloy

By using the interface layer prelithiation drying process of lithium-containing multi-alloy in lithium-ion batteries, the problem of difficulty in controlling the degree of prelithiation and the use of toxic solvents in the prior art is solved, and the high energy density of the negative electrode of the lithium-ion battery is achieved and cycle performance improvement.

CN119050277AInactive Publication Date: 2024-11-29SHAANXI JINGTAI NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411516704.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing prelithiation technology of negative electrodes of lithium-ion batteries is difficult to accurately control the degree of prelithiation, and requires the use of toxic solvents, which limits its industrial application. At the same time, traditional wet processes are difficult to increase the bulk density of the electrodes.

Method used

The lithium-containing alloy layer prelithiated dry negative electrode preparation method is adopted to prepare a lithium-containing alloy layer by mixing lithium foil and pure metal elements under an inert atmosphere, and combining it with the negative electrode material and conductive agent through a dry process to form a High load self-supporting electrode diaphragm achieves controllable prelithiation.

Benefits of technology

Controllable and uniform prelithiation of the negative electrode of the lithium-ion battery in a high humidity environment is achieved, the energy density and circulation performance of the battery are improved, and the limitation of using toxic solvents is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050277A_ABST
    Figure CN119050277A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an interface layer pre-lithiation dry-method negative electrode of a lithium-containing multi-element alloy, and belongs to the technical field of pre-lithiation. Firstly, lithium foil and pure metal elements are subjected to high-temperature roasting to obtain a lithium-containing alloy material, and a lithium-containing alloy layer with the controllable thickness is obtained through rolling; the preparation method comprises the following steps: fibration of polystyrene butadiene rubber is realized through physical modification, then a negative electrode material, a conductive agent and the modified polystyrene butadiene rubber are mixed and added into an ultra-high-speed stirrer for fibration, and fibration powder is repeatedly rolled to form self-supporting electrode diaphragms with different surface capacities; and finally, the lithium-containing alloy layer and the high-load electrode are subjected to rolling compounding to obtain the lithium-containing alloy pre-lithiation negative electrode. According to the preparation method of the interface layer pre-lithiation dry method negative electrode of the lithium-containing multi-element alloy, a high-load and high-first-effect pre-lithiation electrode is prepared under the condition of no organic solvent, and high battery energy density is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pre-lithiation, and in particular to a method for preparing a pre-lithiation dry-process negative electrode of an interface layer containing a lithium multi-element alloy. Background Art

[0002] Since its commercialization in the 1990s, lithium-ion batteries have greatly changed our lives and accelerated the transition from oil- and gas-powered vehicles to pure electric vehicles. Currently, the large-scale industrialization of pure electric vehicles still faces the problems of "charging anxiety", "range anxiety" and high costs. Among them, how to significantly improve the rate performance and energy density of lithium-ion batteries has attracted the most attention of researchers.

[0003] At present, the low theoretical capacity (372mAh / g) of commercial lithium-ion battery graphite negative electrode materials is not enough to meet our demand for high-capacity power batteries. The commercialization of batteries requires improving the energy density of batteries while ensuring economy and safety.

[0004] Silicon is abundant and widely distributed in the earth's crust, and has a slightly higher potential platform than graphite (0.4V vs. Li / Li + ), there is no hidden danger of lithium deposition, good safety, and the highest theoretical specific capacity can reach 4200mAh / g, which is considered to be one of the most promising negative electrode materials. However, silicon negative electrode materials will undergo nearly 300% volume expansion during the process of lithium insertion and extraction, resulting in problems such as particle crushing, electrical isolation and unstable growth of SEI, which will lead to irreversible loss of active lithium and attenuation of cycle performance.

[0005] Pre-lithiation technology is an effective method to solve the ion loss of negative electrode materials in lithium-ion batteries. Currently, the commonly used negative electrode pre-lithiation methods are divided into the following categories: electrochemical pre-lithiation, lithium foil pre-lithiation, stable metal lithium powder (SLMP), chemical pre-lithiation and additive pre-lithiation.

[0006] Electrochemical pre-lithiation mainly controls the degree of pre-lithiation by controlling the cut-off potential and current density, but this method requires repeated disassembly and assembly of the battery, which limits its industrial application. Lithium foil pre-lithiation refers to the direct contact between the electrode and lithium foil in an electrolyte environment. The difference in potential difference causes the directional movement of electron flow, and the Li generated in the lithium foil + is released into the electrolyte. To maintain charge balance, the Li + Insertion / embedding into the negative electrode material to replenish the irreversible lithium loss and achieve high coulombic efficiency and cycle life. Although this pre-lithiation method has the advantages of high efficiency and easy preparation, it is difficult to accurately control the degree of pre-lithiation.

[0007] Stable metallic lithium powder, chemical pre-lithiation and additive pre-lithiation can all replenish lithium to the stacked negative electrode, but they all require the use of toxic solvents and have extremely stringent environmental requirements, which restricts their industrial application. In addition, the traditional wet coating process has reached its limit in improving the volume density of the electrode, and there is an urgent need to develop a new electrode preparation process. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a pre-lithiation dry-process negative electrode of an interface layer containing a lithium multi-element alloy, so as to solve the problem that the existing pre-lithiation technology is difficult to accurately control the degree of pre-lithiation and requires the use of toxic solvents, thereby limiting its industrial application. At the same time, the volume density of the electrode is improved to achieve controllable and uniform pre-lithiation of the negative electrode of a lithium-ion battery in a high-humidity environment.

[0009] To achieve the above object, the present invention provides a method for preparing a pre-lithiated dry-process negative electrode of an interface layer containing a lithium multi-element alloy, comprising the following steps: S1. In an inert atmosphere, lithium foil and pure metal elements are uniformly mixed according to a mass ratio, spread flat on a stainless steel boat, and heated and stirred to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material is placed in a drying room with a relative humidity of less than 15% and thinned using a roller press to obtain a lithium-containing alloy layer; S2, dissolving polystyrene butadiene rubber SBR in an organic solvent, adding the obtained mixed solution dropwise to an inorganic salt, stirring at room temperature and then drying, then repeatedly washing with water and anhydrous ethanol for 3-10 times, and drying the washed material to obtain a modified SBR; S3, stirring the negative electrode material, the conductive agent and the modified SBR at ultra-high speed to obtain a pole piece powder; repeatedly rolling the pole piece powder to form a self-supporting electrode membrane; thermally compounding the self-supporting electrode membrane with Cu foil, and rolling forming to obtain a high-load dry-process negative electrode; S4, rolling the lithium-containing alloy layer obtained in S1 and the high-load dry-process negative electrode obtained in S3 to obtain a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy.

[0010] Preferably, the pure metal elements in S1 are any two of Mg, Al, Zn, Sn, Ag, Cr, and Ti, and the mass ratio of lithium foil to any two of the pure metal elements is 10:(0.1-3):(0.1-3).

[0011] Preferably, the heating temperature in S1 is 200-500° C., the stirring time is 5-12 h, and the thickness of the lithium alloy layer is 2-50 μm.

[0012] Preferably, the organic solvent in S2 is one or more of p-xylene, N-methylpyrrolidone, N,N-dimethylformamide, toluene, tetrahydrofuran, hexane, cyclohexane, methyl formate, ethyl acetate, dichloromethane, and 1,3-dioxolane, and the inorganic salt is one or more of NaCl, KCl, Na2CO3, K2CO3, and MgCl2.

[0013] Preferably, the mass ratio of the mixed solution to the inorganic salt in S2 is 1:(20-35), the stirring time is 5-12h, the first drying temperature is 80-180°C, the drying time is 8-48h, and the second drying temperature is 60-120°C, and the drying time is 6-12h.

[0014] Preferably, the negative electrode material in S3 is one or more of silicon-carbon material, silicon-oxygen material, graphite, tin powder, and hard carbon, and the conductive agent is one or more of conductive carbon black, carbon fiber, conductive graphite, single-walled carbon nanotube, and vapor-grown carbon fiber.

[0015] Preferably, the ratio of the negative electrode material, the conductive agent and the modified SBR in the S3 is (70-90%): (5-20%): (5-10%), the stirring speed of the ultra-high-speed stirring is 1000-20000 rpm / min, and the stirring time is 10-50 min.

[0016] Preferably, the temperature of rolling the electrode powder in S3 is 80-150°C, and the surface capacity of the self-supporting electrode membrane is 4-10 mAh / cm 2 .

[0017] Preferably, the compounding condition in S3 is: roll-to-roll thermal compounding at 80-180°C.

[0018] Therefore, the present invention adopts the above-mentioned method for preparing a pre-lithiated dry-process negative electrode of the interface layer containing a lithium multi-element alloy, and the present invention has the following technical effects: (1) preparing a lithium-containing alloy material by calcining lithium metal and pure metal powder, and achieving a controllable thickness of a lithium-containing alloy layer by repeated rolling; (2) A high-load lithium alloy layer negative electrode (>8 mAh / cm 2 ), which can effectively improve the energy density of the battery.

[0019] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The TEM image of 96Li2Mg2Al alloy particles prepared in Example 1 of the method for preparing a pre-lithiation dry-process negative electrode of an interface layer containing a lithium multi-element alloy; Figure 2 A method for preparing a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy Example 1 96Li2Mg2Al-SiO x @C cross-sectional SEM image of the negative electrode; Figure 3 It is a preparation method of a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy. Effect Example 1: The first cycle charge and discharge curve of the assembled button half-cell; Figure 4 It is a preparation method of a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy. Effect Example 2 The first cycle charge and discharge curve of the assembled button half-cell; Figure 5 It is a preparation method of a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy. Effect Example 3 The first cycle charge and discharge curve of the assembled button half-cell; Figure 6 It is a preparation method of a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy. Effect Example 4 The first cycle charge and discharge curve of the assembled button half-cell; Figure 7 It is a preparation method of a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy. Effect Example 5 The first cycle charge and discharge curve of the assembled button half-cell; Figure 8 The invention relates to a method for preparing a dry-process negative electrode having an interface layer pre-lithiation containing a lithium multi-element alloy. Example 1 shows the capacity retention rate of a button-type half-battery prepared during 100 cycles. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0022] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0023] Example The present invention provides a method for preparing a pre-lithiated dry-process negative electrode of an interface layer containing a lithium multi-element alloy, comprising the following steps: S1. In an inert atmosphere, lithium foil and pure metal elements are mixed evenly, spread flat in a stainless steel boat, heated to 200-500°C, stirred for 5-12 hours to obtain a lithium-containing alloy material, and the cooled lithium-containing alloy material is thinned to 2-50 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer. The lithium foil is commercial lithium foil, the pure metal elements are any two of Mg, Al, Zn, Sn, Ag, Cr, and Ti, and the mass ratio of lithium foil to any two of the pure metal elements is 10:(0.1-3):(0.1-3).

[0024] S2. Dissolve polystyrene butadiene rubber SBR in an organic solvent, add the resulting mixed solution dropwise to an inorganic salt at a mass ratio of 1:(20-35), stir at room temperature for 5-12 hours, and then dry at 80-180°C for 8-48 hours to remove the organic solvent, then wash repeatedly with water and anhydrous ethanol for 3-10 times, and dry the washed material at 60-120°C for 6-12 hours to obtain modified SBR. Stirring can enable SBR to achieve fiberization under high-speed shear force.

[0025] The organic solvent is one or more of p-xylene, N-methylpyrrolidone, N,N-dimethylformamide, toluene, tetrahydrofuran, hexane, cyclohexane, methyl formate, ethyl acetate, dichloromethane, and 1,3-dioxolane, and the inorganic salt is one or more of NaCl, KCl, Na2CO3, K2CO3, and MgCl2.

[0026] S3, 70-90% negative electrode material, 5-20% conductive agent and 5-10% modified SBR are stirred at a speed of 1000-20000 rpm for 10-50 min to obtain a pole piece powder; the pole piece powder is repeatedly rolled at 80-150°C to form a surface capacity of 4-10 mAh / cm 2 A self-supporting electrode membrane is prepared; the self-supporting electrode membrane is roll-to-roll thermally composited with Cu foil at 80-180°C, and a high-load dry-process negative electrode is obtained after roll-forming.

[0027] The negative electrode material, the conductive agent and the modified SBR form a binder, which is fiberized by ultra-high-speed stirring. The negative electrode material is one or more of silicon-carbon material, silicon-oxygen material, graphite, tin powder and hard carbon, and the conductive agent is one or more of conductive carbon black, carbon fiber, conductive graphite, single-walled carbon nanotube and vapor-grown carbon fiber.

[0028] S4, rolling the lithium-containing alloy layer obtained in S1 and the high-load dry-process negative electrode obtained in S3 to obtain a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy.

[0029] Example 1 A method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy comprises the following steps: S1. Under an inert atmosphere, commercial lithium foil was mixed with Mg powder and Al powder in a mass ratio of 10:1:1, spread in a stainless steel boat, heated to 200°C, and stirred for 5 hours to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material was thinned to a thickness of 5 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer, which was recorded as 96Li2Mg2Al.

[0030] S2. Dissolve polystyrene butadiene rubber in p-xylene, add the resulting mixed solution dropwise into NaCl at a mass ratio of 1:35, stir at room temperature for 5 hours, and then dry at 80°C for 8 hours to remove the p-xylene, then repeatedly wash the dried product with water and anhydrous ethanol for 3 times, and dry the washed material at 60°C for 6 hours to obtain modified SBR.

[0031] S3, 70% silicon oxide material, 20% conductive carbon black, and 10% modified SBR were stirred at 1000 rpm for 20 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 80°C to form a surface capacity of 4 mAh / cm 2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 80°C, and a high-load dry silicon oxide negative electrode is obtained after roll-forming.

[0032] S4, further rolling the lithium-containing alloy layer obtained in S1 and the high-load dry-process silicon-oxygen negative electrode obtained in S3 to obtain a high-load pre-lithiated silicon-oxygen negative electrode, denoted as 96Li2Mg2Al-SiO x @C.

[0033] Figure 1 This is a high-resolution image of the 96Li2Mg2Al alloy particles prepared in this example observed under a transmission electron microscope. Figure 1 It can be seen that there are Li-Al-O, MgO and Al2O3 crystal planes in the 96Li2Mg2Al alloy particles, which proves the formation of 96Li2Mg2Al alloy particles, and the thickness of the 96Li2Mg2Al alloy layer is 5μm. Figure 2 96Li2Mg2Al-SiO prepared in this example x @C electrode SEM cross-sectional view, it can be seen that 96Li2Mg2Al-SiO x @C clearly has a two-layer structure with a total thickness of 20 μm.

[0034] Example 2 A method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy comprises the following steps: S1. Under an inert atmosphere, commercial lithium foil was mixed with Zn powder and Ag powder in a mass ratio of 10:0.5:1, spread on a stainless steel boat, heated to 300°C, and stirred for 12 hours to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material was thinned to a thickness of 10 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer.

[0035] S2. Dissolve polystyrene butadiene rubber in N-methylpyrrolidone, add the resulting mixed solution dropwise into KCl at a mass ratio of 1:20, stir at room temperature for 12 hours, and then dry at 120°C for 24 hours to remove N-methylpyrrolidone, then repeatedly wash the dried product with water and anhydrous ethanol for 5 times, and dry the washed material at 80°C for 10 hours to obtain modified SBR.

[0036] S3, 90% silicon oxide material, 5% conductive carbon black, and 5% modified SBR were stirred at 2000 rpm for 20 minutes to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 80°C to form a surface capacity of 8 mAh / cm 2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 90°C, and a high-load dry silicon oxide negative electrode is obtained after roll-forming.

[0037] S4, further rolling the lithium-containing alloy layer obtained in S1 and the high-load dry-process silicon-oxygen negative electrode obtained in S3 to obtain a high-load pre-lithiated silicon-oxygen negative electrode.

[0038] Example 3 A method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy comprises the following steps: S1. Under an inert atmosphere, commercial lithium foil was mixed with Ag powder and Al powder in a mass ratio of 10:1:1, spread on a stainless steel boat, heated to 350°C, and stirred for 6 hours to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material was thinned to a thickness of 5 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer.

[0039] S2. Dissolve polystyrene butadiene rubber in N,N-dimethylformamide, add the resulting mixed solution dropwise into Na2CO3 at a mass ratio of 1:35, stir at room temperature for 8 hours, and then dry at 180°C for 36 hours to remove N,N-dimethylformamide, then repeatedly wash the dried product with water and anhydrous ethanol 10 times, and dry the washed material at 100°C for 9 hours to obtain modified SBR.

[0040] S3, 80% silicon carbon material, 10% vapor-grown carbon fiber, and 10% modified SBR were stirred at 1500 rpm for 30 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 120°C to form a surface capacity of 7 mAh / cm 2 A self-supporting electrode membrane is prepared; the self-supporting electrode membrane is thermally composited with Cu foil at 120°C by roll-to-roll process, and a high-load dry silicon-carbon negative electrode is obtained after roll-forming.

[0041] S4. The lithium-containing alloy layer obtained in S1 and the high-load dry silicon-carbon negative electrode obtained in S3 are further rolled to obtain a high-load pre-lithiation silicon-carbon negative electrode.

[0042] Example 4 A method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy comprises the following steps: S1. Under an inert atmosphere, commercial lithium foil was mixed with Al powder and Ag powder in a mass ratio of 10:1:0.5, spread on a stainless steel boat, heated to 450°C, and stirred for 10 hours to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material was thinned to a thickness of 10 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer.

[0043] S2. Dissolve polystyrene butadiene rubber in toluene, add the resulting mixed solution dropwise into NaCl at a mass ratio of 1:35, stir at room temperature for 5 hours, and then dry at 80°C for 8 hours to remove toluene, then repeatedly wash the dried product with water and anhydrous ethanol for 3 times, and dry the washed material at 60°C for 6 hours to obtain modified SBR.

[0044] S3, 70% silicon carbon material, 20% single-walled carbon nanotubes, and 10% modified SBR were stirred at 1000 rpm for 20 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 80°C to form a surface capacity of 4 mAh / cm 2 A self-supporting electrode membrane is prepared; the self-supporting electrode membrane is roll-to-roll thermally composited with Cu foil at 80°C, and a high-load dry silicon-carbon negative electrode is obtained after roll-forming.

[0045] S4. The lithium-containing alloy layer obtained in S1 and the high-load dry silicon-carbon negative electrode obtained in S3 are further rolled to obtain a high-load pre-lithiation silicon-carbon negative electrode.

[0046] Example 5 A method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy comprises the following steps: S1. Under an inert atmosphere, commercial lithium foil was mixed with Mg powder and Al powder in a mass ratio of 10:1:1, spread on a stainless steel boat, heated to 200°C, and stirred for 5 hours to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material was thinned to a thickness of 5 μm using a roller press in a drying room with a relative humidity of less than 15% to obtain a lithium-containing alloy layer.

[0047] S2. Dissolve polystyrene butadiene rubber in 1,3-dioxolane, add the resulting mixed solution dropwise into MgCl2 at a mass ratio of 1:35, stir at room temperature for 5 hours, and then dry at 80°C for 8 hours to remove 1,3-dioxolane, then repeatedly wash the dried product with water and anhydrous ethanol for 3 times, and dry the washed material at 60°C for 6 hours to obtain modified SBR.

[0048] S3, 80% tin powder, 10% carbon fiber, and 10% modified SBR were stirred at 1800 rpm for 20 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 150°C to form a surface capacity of 6 mAh / cm 2 A self-supporting electrode membrane is prepared; the self-supporting electrode membrane is roll-to-roll thermally composited with Cu foil at 150°C, and a high-load dry-process Sn-based negative electrode is obtained after roll-forming.

[0049] S4, further rolling the lithium-containing alloy layer in S1 and the high-load dry silicon-carbon negative electrode in S3 to obtain a high-load pre-lithiated Sn-based negative electrode.

[0050] Comparative Example 1 Polystyrene butadiene rubber was dissolved in p-xylene, and the resulting mixed solution was added dropwise into NaCl at a mass ratio of 1:35. After stirring at room temperature for 5 hours, the mixture was dried at 80°C for 8 hours to remove the p-xylene. The dried product was then repeatedly washed three times with water and anhydrous ethanol, and the washed material was dried at 60°C for 6 hours to obtain the modified SBR.

[0051] 70% silicon oxide material, 20% conductive carbon black and 10% modified SBR were stirred at 1000 rpm for 20 min to obtain the electrode powder; the electrode powder was repeatedly rolled at 80°C to form a surface capacity of 4 mAh / cm 2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 80°C, and a non-pre-lithiated silicon-oxygen negative electrode is obtained after roll-forming.

[0052] Comparative Example 2 Polystyrene butadiene rubber was dissolved in N-methylpyrrolidone, and the obtained mixed solution was added dropwise into KCl at a mass ratio of 1:20. After stirring at room temperature for 12 hours, it was dried at 120°C for 24 hours to remove N-methylpyrrolidone. The dried product was then repeatedly washed 5 times with water and anhydrous ethanol, and the washed material was dried at 80°C for 10 hours to obtain modified SBR.

[0053] 90% silicon oxide material, 5% conductive carbon black and 5% modified SBR were stirred at 2000 rpm for 20 min to obtain the electrode powder; the electrode powder was repeatedly rolled at 80°C to form a surface capacity of 8 mAh / cm2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 90°C, and a non-pre-lithiated silicon-oxygen negative electrode is obtained after roll-forming.

[0054] Comparative Example 3 Polystyrene butadiene rubber was dissolved in N,N-dimethylformamide, and the obtained mixed solution was added dropwise into Na2CO3 at a mass ratio of 1:35. After stirring at room temperature for 8 hours, it was dried at 180°C for 36 hours to remove N,N-dimethylformamide. The dried product was then repeatedly washed 10 times with water and anhydrous ethanol, and the washed material was dried at 100°C for 9 hours to obtain modified SBR.

[0055] 80% silicon carbon material, 10% vapor-grown carbon fiber, and 10% modified SBR were stirred at 1500 rpm for 30 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 120°C to form a surface capacity of 7 mAh / cm 2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 120°C, and a non-pre-lithiation silicon-carbon negative electrode is obtained after roll-forming.

[0056] Comparative Example 4 Polystyrene butadiene rubber was dissolved in toluene, and the obtained mixed solution was added dropwise into NaCl at a mass ratio of 1:35. After stirring at room temperature for 5 hours, it was dried at 80°C for 8 hours to remove the toluene. The dried product was then repeatedly washed three times with water and anhydrous ethanol, and the washed material was dried at 60°C for 6 hours to obtain the modified SBR.

[0057] 70% silicon carbon material, 20% single-walled carbon nanotubes, and 10% modified SBR were stirred at 1000 rpm for 20 min to obtain a pole piece powder; the pole piece powder was repeatedly rolled at 80°C to form a surface capacity of 4 mAh / cm 2 A self-supporting electrode membrane; the self-supporting electrode membrane and Cu foil are roll-to-roll thermally composited at 80°C, and a non-pre-lithiation silicon-carbon negative electrode is obtained after roll-forming.

[0058] Comparative Example 5 Polystyrene butadiene rubber was dissolved in 1,3-dioxolane, and the resulting mixed solution was added dropwise into MgCl2 at a mass ratio of 1:35. After stirring at room temperature for 5 hours, the mixture was dried at 80°C for 8 hours to remove 1,3-dioxolane. The dried product was then washed repeatedly three times with water and anhydrous ethanol, and the washed material was dried at 60°C for 6 hours to obtain modified SBR.

[0059] 80% tin powder, 10% carbon fiber, and 10% modified SBR were stirred at 1800 rpm for 20 min to obtain a pole piece powder. The pole piece powder was repeatedly rolled at 150°C to form a surface capacity of 6 mAh / cm 2 A self-supporting electrode membrane is prepared; the self-supporting electrode membrane is roll-to-roll thermally composited with Cu foil at 150° C., and a non-pre-lithiated Sn-based negative electrode is obtained after roll-forming.

[0060] Effect Example 1 The button half-cells were assembled using the high-load pre-lithiated silicon oxide negative electrode prepared in Example 1 and the non-pre-lithiated silicon oxide negative electrode prepared in Comparative Example 1, that is, the positive electrode shell, the high-load pre-lithiated negative electrode / non-pre-lithiated negative electrode, the separator, the lithium foil, the gasket and the negative electrode shell were placed in sequence. The electrolyte was prepared by a volume ratio of 3:4:3 of ethylene carbonate: dimethyl carbonate: diethylene carbonate, and 5wt% of FEC and 1mol / L of LiPF6 were added.

[0061] Effect Example 2 The button-type half-cells were assembled using the high-load pre-lithiated silicon oxide negative electrode prepared in Example 2 and the non-pre-lithiated silicon oxide negative electrode prepared in Comparative Example 2, that is, the positive electrode shell, the high-load pre-lithiated negative electrode / non-pre-lithiated negative electrode, the separator, the lithium foil, the gasket and the negative electrode shell were placed in sequence. The electrolyte was prepared by a volume ratio of 3:4:3 of ethylene carbonate: dimethyl carbonate: diethylene carbonate, and 5wt% of FEC and 1mol / L of LiPF6 were added.

[0062] Effect Example 3 The button-type half-cells were assembled using the high-load pre-lithiated silicon-carbon anode prepared in Example 3 and the non-pre-lithiated silicon-carbon anode prepared in Comparative Example 3, that is, the positive electrode shell, the high-load pre-lithiated anode / non-pre-lithiated anode, the separator, the lithium foil, the gasket and the negative electrode shell were placed in sequence. The electrolyte was prepared by a volume ratio of 3:4:3 of ethylene carbonate: dimethyl carbonate: diethylene carbonate, and 5wt% of FEC and 1mol / L of LiPF6 were added.

[0063] Effect Example 4 The button-type half-cells were assembled using the high-load pre-lithiation silicon-carbon anode prepared in Example 4 and the non-pre-lithiation silicon-carbon anode prepared in Comparative Example 4, that is, the positive electrode shell, the high-load pre-lithiation anode / non-pre-lithiation anode, the separator, the lithium foil, the gasket and the negative electrode shell were placed in sequence. The electrolyte was prepared by a volume ratio of 3:4:3 of ethylene carbonate: dimethyl carbonate: diethylene carbonate, and 5wt% of FEC and 1mol / L of LiPF6 were added.

[0064] Effect Example 5 The button-type half-cells were assembled using the high-load pre-lithiated Sn-based negative electrode prepared in Example 5 and the non-pre-lithiated Sn-based negative electrode prepared in Comparative Example 5, that is, the positive electrode shell, the high-load pre-lithiated negative electrode / non-pre-lithiated negative electrode, the separator, the lithium foil, the gasket and the negative electrode shell were placed in sequence. The electrolyte was prepared by a volume ratio of 3:4:3 of ethylene carbonate: dimethyl carbonate: diethylene carbonate, and 5wt% of FEC and 1mol / L of LiPF6 were added.

[0065] Experimental Testing The Xinwei test cabinet CT-4000 was used to perform the test in the voltage range of 0.05~1.5V using the constant current and constant voltage charge and discharge method.

[0066] (1) The first cycle charge and discharge curves of button-type half-cells assembled in Example 1 to 5 are as follows: Figures 3~8 shown.

[0067] Depend on Figure 3 It can be seen that compared with the non-pre-lithiated silicon oxide negative electrode in comparative example 1, the lithium insertion / delithiation capacity of the high-load pre-lithiated silicon oxide negative electrode in embodiment 1 decreased from 2051.6 / 1546 mAh / g to 1457.5 / 1324 mAh / g, and the first-week efficiency increased from 75.3% to 90.4%.

[0068] Depend on Figure 4 It can be seen that compared with the non-pre-lithiated silicon oxide negative electrode in comparative example 2, the lithium insertion capacity of the high-load pre-lithiated silicon oxide negative electrode in embodiment 2 is reduced from 2045.4 / 1543.2 mAh / g to 1562.6 / 1362.5 mAh / g, and the first-week efficiency is increased from 75.4% to 87.2%.

[0069] Depend on Figure 5 It can be seen that compared with the non-pre-lithiated silicon-carbon negative electrode in comparative example 3, the lithium insertion capacity of the high-load pre-lithiated silicon-carbon negative electrode in embodiment 3 decreased from 1607.8.6 mAh / g to 1516.9 mAh / g, and the first-week efficiency increased from 62.3% to 71.4%.

[0070] Depend on Figure 6 It can be seen that compared with the non-pre-lithiated silicon-carbon negative electrode in Comparative Example 4, the lithium insertion capacity of the high-load pre-lithiated silicon-carbon negative electrode in Example 4 decreased from 2164.4 mAh / g to 2044.9 mAh / g, and the first-week efficiency increased from 70.4% to 87.5%.

[0071] Depend on Figure 7 It can be seen that compared with the non-pre-lithiated Sn-based negative electrode in comparative example 5, the lithium insertion capacity of the high-load pre-lithiated Sn-based negative electrode in embodiment 5 is reduced from 1185 mAh / g to 660 mAh / g, and the first-cycle efficiency is increased from 62.5% to 112.3%.

[0072] (2) The capacity retention rate of the button-type half-cell prepared in Example 1 during 100 cycles is as follows: Figure 8 It can be concluded that compared with the non-pre-lithiation silicon oxide negative electrode in comparative example 1 (the capacity retention rate after 100 cycles is 50.4%), the capacity retention rate of the high-load pre-lithiation silicon oxide negative electrode in example 1 after 100 cycles is 87%, indicating that the pre-lithiation treatment operation in example 1 is beneficial to improving the electrochemical performance of the negative electrode.

[0073] Therefore, the present invention adopts the above-mentioned method for preparing a pre-lithiation dry-process negative electrode with an interface layer containing a lithium multi-element alloy to solve the problem that the existing pre-lithiation technology is difficult to accurately control the degree of pre-lithiation and requires the use of toxic solvents, thereby limiting its industrial application. At the same time, the volume density of the electrode is improved to achieve controllable and uniform pre-lithiation of the negative electrode of the lithium-ion battery in a high humidity environment.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy, It is characterized in that The following steps are involved: S1. In an inert atmosphere, lithium foil and pure metal elements are uniformly mixed according to a mass ratio, spread flat on a stainless steel boat, and heated and stirred to obtain a lithium-containing alloy material. The cooled lithium-containing alloy material is placed in a drying room with a relative humidity of less than 15% and thinned using a roller press to obtain a lithium-containing alloy layer; S2, dissolving polystyrene butadiene rubber SBR in an organic solvent, adding the obtained mixed solution dropwise to an inorganic salt, stirring at room temperature and then drying, then repeatedly washing with water and anhydrous ethanol for 3-10 times, and drying the washed material to obtain a modified SBR; S3, stirring the negative electrode material, the conductive agent and the modified SBR at ultra-high speed to obtain a pole piece powder; repeatedly rolling the pole piece powder to form a self-supporting electrode membrane; thermally compounding the self-supporting electrode membrane with Cu foil, and rolling forming to obtain a high-load dry-process negative electrode; S4, rolling the lithium-containing alloy layer obtained in S1 and the high-load dry-process negative electrode obtained in S3 to obtain a pre-lithiated dry-process negative electrode with an interface layer containing a lithium multi-element alloy.

2. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The pure metal elements in S1 are any two of Mg, Al, Zn, Sn, Ag, Cr, and Ti, and the mass ratio of lithium foil to any two of the pure metal elements is 10:(0.1-3):(0.1-3).

3. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that In the S1, the heating temperature is 200-500° C., the stirring time is 5-12 hours, and the thickness of the lithium alloy layer is 2-50 μm.

4. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The organic solvent in S2 is one or more of p-xylene, N-methylpyrrolidone, N,N-dimethylformamide, toluene, tetrahydrofuran, hexane, cyclohexane, methyl formate, ethyl acetate, dichloromethane, and 1,3-dioxolane, and the inorganic salt is NaCl, KCl, Na 2 CO 3 , K 2 CO 3 MgCl 2 One or more of .

5. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The mass ratio of the mixed solution to the inorganic salt in S2 is 1:(20-35), the stirring time is 5-12 hours, the first drying temperature is 80-180°C, the drying time is 8-48 hours, the second drying temperature is 60-120°C, and the drying time is 6-12 hours.

6. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The negative electrode material in S3 is one or more of silicon-carbon material, silicon-oxygen material, graphite, tin powder, and hard carbon, and the conductive agent is one or more of conductive carbon black, carbon fiber, conductive graphite, single-walled carbon nanotube, and vapor-grown carbon fiber.

7. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The ratio of the negative electrode material, the conductive agent and the modified SBR in the S3 is (70-90%): (5-20%): (5-10%), the stirring speed of the ultra-high-speed stirring is 1000-20000 rpm / min, and the stirring time is 10-50 min.

8. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The temperature of rolling the electrode powder in S3 is 80-150°C, and the surface capacity of the self-supporting electrode membrane is 4-10 mAh / cm 2 .

9. The method for preparing a pre-lithiated dry-process negative electrode having an interface layer containing a lithium multi-element alloy according to claim 1, It is characterized in that The compounding conditions in S3 are: roll-to-roll thermal compounding at 80-180°C.

Citation Information

Patent Citations

  • Method for enhancing styrene butadiene rubber through basic magnesium chloride crystal whiskers

    CN105440363A

  • Ultrathin lithium-silver alloy strip for lithium ion battery anode and preparation method thereof

    CN110265654A

  • Preparation method of lithium-silicon alloy pole piece, lithium-silicon alloy pole piece and lithium battery

    CN113690427A

  • Method for preparing pre-lithiated negative electrode, pre-lithiated negative electrode and secondary battery

    CN115642228A

  • Lithium supplement negative plate, preparation method thereof and battery

    CN115763700A

Cited By

  • Pre-lithiated negative pole piece, preparation method of lithium supplementing composite layer, lithium supplementing method, secondary battery and electronic device

    CN119920904A

  • Pre-lithiated silicon-based negative electrode, dry preparation method thereof and application of pre-lithiated silicon-based negative electrode in solid-state lithium battery

    CN120749121A