Iodine-doped nano molybdenum disulfide composite carbon material as well as preparation method and application thereof

Through iodine-doped and amorphous carbon-covered nanomolybdenum disulfide materials, the poor conductivity and structural instability of molybdenum disulfide in sodium ion batteries are solved, and efficient sodium ion electrochemical storage is achieved, and electrochemical performance is improved. and cycle life.

CN119050305APending Publication Date: 2024-11-29QINGDAO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160319.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing molybdenum disulfide materials have problems such as poor conductivity, slow reaction kinetics, severe volume expansion and structural instability in sodium ion batteries, which limit their application in sodium ion batteries.

Method used

Through the preparation method of iodine-doped nanomolybdenum disulfide composite carbon material, iodine doping is used to achieve a stable phase transition from 2H to 1T phase, combined with amorphous carbon coverage, the conductivity and structural stability of the material are improved.

Benefits of technology

It has achieved high discharge capacity, excellent rate capability and long cycle life, and improved the electrochemical performance of molybdenum disulfide material. It is specifically manifested as the specific capacity is increased to 550mAh g-1 under the current density of 3Ag-1, and the rate performance is also significantly promote.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050305A_ABST
    Figure CN119050305A_ABST
Patent Text Reader

Abstract

The invention discloses an iodine-doped nano molybdenum disulfide composite carbon material as well as a preparation method and application thereof, and belongs to the field of molybdenum disulfide catalytic materials. The three-dimensional nano-flower structure comprises iodine-doped nano-molybdenum disulfide sheets and amorphous carbon, the iodine-doped nano-molybdenum disulfide sheets are stacked into a three-dimensional nano-flower structure, and the amorphous carbon covers the surfaces of the iodine-doped nano-molybdenum disulfide sheets. The iodide ions induce the 2H-MoS2 to be stably changed into the 1T-MoS2 in a phase mode, meanwhile, amorphous carbon is inserted between molybdenum disulfide single layers, the atom-interface interaction between the amorphous carbon and the molybdenum disulfide single layers avoids re-accumulation of the molybdenum disulfide single layers, and the electrochemical performance of molybdenum disulfide is improved. Compared with a blank sample material, the iodine-doped molybdenum disulfide material can reach the specific capacity of 550mAh g <-1 > under the current density of 3Ag <-1 >, the specific capacity of a blank sample is 400mAh g <-1 >, and compared with the blank sample material, the rate capability is also improved to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of molybdenum disulfide catalytic materials, and specifically relates to an iodine-doped nano molybdenum disulfide composite carbon material and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Lithium-ion batteries (LIBs) are the most widely used type of battery in current energy storage technology. Due to the relative scarcity of lithium resources, the cost of LIBs is relatively high, which limits the large-scale application of LIBs. Sodium is the fourth most abundant element in the earth's crust, and its resources are far more abundant than lithium. Sodium and lithium are elements of the same main group, and the two have similar physical and chemical properties. Therefore, it is feasible to use sodium ions instead of lithium ions as secondary batteries. However, the radius of sodium ions is Larger MoS leads to severe volume expansion and slow transport kinetics, resulting in low reversible capacity and rapid capacity decay in sodium ion batteries. 2 It has a unique layered structure, a large interlayer distance (0.62nm), and a high theoretical specific capacity (670mAhg -1 However, as the negative electrode material of sodium ion batteries, it still has serious problems, including poor conductivity during electroosmosis, slow reaction kinetics, severe volume expansion, polysulfide shuttle, etc., which lead to unsatisfactory electrochemical performance and limit the application of MoS 2 Therefore, it will be of great research value and significance to obtain high-performance molybdenum-based sulfide anode materials through reasonable and effective design and preparation methods to achieve efficient and stable sodium electrochemical storage.

[0004] Based on the different coordination forms of Mo and S atoms, MoS2 exhibits trigonal prismatic 2H phase and octahedral coordinated 1T phase. Thermodynamically stable 2H phase MoS2 (2H-MoS 2 ), the semiconductor properties show poor conductivity. 2 In addition, the distorted octahedral coordination makes 1T-MoS 2 With a larger interlayer spacing, it is more favorable for Na + However, 1T-MoS 2The structural stability is poor, and there are still some inherent limitations, such as complex synthesis process and difficult reaction control, which limit its practical application. Patent CN117963988A discloses a method for preparing defective molybdenum disulfide that promotes phase transition from 2H to 1T by Co doping. The defects are introduced by introducing Co atoms to activate the inert basal plane of molybdenum disulfide, while promoting the generation of more stable 1T phases and improving the conductivity, so as to serve as a bifunctional electrode material for aqueous sulfur-iodine flow batteries. This provides a strategy for molybdenum disulfide materials to achieve a stable phase transition from 2H to 1T. Therefore, there is an urgent need to develop a method for achieving a stable phase transition from 2H to 1T to obtain molybdenum disulfide electrode materials suitable for sodium ion batteries. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide an iodine-doped nano-molybdenum disulfide composite carbon material and a preparation method and application thereof. The iodine-doped nano-molybdenum disulfide composite carbon material provided by the present invention effectively realizes a stable phase transition from 2H to 1T.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] The first aspect of the present invention provides an iodine-doped nano-molybdenum disulfide composite carbon material, comprising iodine-doped nano-molybdenum disulfide sheets and amorphous carbon, wherein the iodine-doped nano-molybdenum disulfide sheets are stacked into a three-dimensional nanoflower structure, and the amorphous carbon covers the surface of the iodine-doped nano-molybdenum disulfide sheets.

[0008] In some embodiments of the present invention, the nano-molybdenum disulfide includes 2H phase molybdenum disulfide and 1T phase molybdenum disulfide.

[0009] The second aspect of the present invention provides a method for preparing the iodine-doped nano-molybdenum disulfide composite carbon material, comprising the following steps:

[0010] At room temperature, a carbon source is dissolved in water, and then a molybdenum source, a sulfur source, and finally an iodine source are added in sequence to obtain a mixed solution;

[0011] The obtained mixed solution is subjected to a hydrothermal reaction to obtain a precursor material;

[0012] The obtained precursor material is calcined under a protective atmosphere to obtain an iodine-doped nano-molybdenum disulfide composite carbon material.

[0013] In some embodiments of the present invention, the carbon source includes glucose, sucrose or citric acid, preferably glucose.

[0014] In some embodiments of the present invention, the molybdenum source includes sodium molybdate or ammonium molybdate, preferably sodium molybdate.

[0015] In some embodiments of the present invention, the sulfur source includes thiourea, sodium thioacetate or ammonium sulfate, preferably thiourea.

[0016] In some embodiments of the present invention, the iodine source is sodium iodide.

[0017] In some embodiments of the present invention, the carbon source is glucose, the molybdenum source is sodium molybdate, the sulfur source is thiourea, and the iodine source is sodium iodate. The present invention selects glucose, sodium molybdate dihydrate, thiourea and sodium iodide as the carbon source, molybdenum source, sulfur source and iodine source, which is simple to prepare and the raw materials are easily available.

[0018] In some embodiments of the present invention, the mass ratio of glucose, sodium molybdate, thiourea and sodium iodide is (0.8-1):1:2:(0.3-0.4), preferably 0.9:1:2:0.3125.

[0019] In some embodiments of the present invention, the hydrothermal reaction has a reaction temperature of 180-220° C. and a reaction time of 20-25 h.

[0020] In some embodiments of the present invention, the precursor material is centrifuged with a washing liquid, dried, and then calcined;

[0021] Preferably, the drying temperature is 50-70°C;

[0022] Preferably, the calcination has a heating rate of 4-6°C / min, a calcination temperature of 480-520°C, and a calcination time of 1.5-2.5h.

[0023] In some embodiments of the present invention, the protective atmosphere is a nitrogen atmosphere or an argon atmosphere, preferably a nitrogen atmosphere.

[0024] A third aspect of the present invention provides a sodium ion battery negative electrode, comprising a current collector, a binder, a conductive agent and a negative electrode active material;

[0025] The binder, the conductive agent and the negative electrode active material are mixed and attached to at least one surface of the current collector;

[0026] The negative electrode active material is the iodine-doped nano-molybdenum disulfide composite carbon material or the iodine-doped nano-molybdenum disulfide composite carbon material prepared by the preparation method.

[0027] A fourth aspect of the present invention provides a sodium ion battery, comprising a positive electrode and a negative electrode, wherein the negative electrode is the negative electrode of the sodium ion battery.

[0028] The beneficial effects of the present invention are:

[0029] The present invention provides an iodine-doped nano-molybdenum disulfide composite carbon material, which achieves a stable phase transition from 2H to 1T through iodine doping, improves the conductivity of the composite material, enhances charge transfer kinetics, reduces ion diffusion barriers, enhances structural stability, and achieves high discharge capacity, excellent rate capability and long cycle life. The present invention adds a polymer containing carbon, molybdenum, sulfur and iodine elements to a precursor solution, hydrothermally synthesizes a carbon-coated nano-molybdenum disulfide material through the precursor solution, and in-situ carbonizes it into amorphous carbon through a one-step method to obtain an iodine-doped carbon-coated molybdenum disulfide material. Iodine ion induces 2H-MoS 2 Stable phase transition to 1T-MoS 2 At the same time, amorphous carbon is inserted between the MoS2 monolayers. The atomic-interface interaction between them avoids the restacking of the MoS2 monolayers and improves the electrochemical performance of MoS2. -1 The specific capacity can reach 550 mAh g -1 The specific capacity of the blank sample is 400 mAh g -1 , compared with the blank sample, the rate performance has also been improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0031] Figure 1 This is a transmission electron microscope image of the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 1 of the present invention;

[0032] Figure 2 The iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 1 of the present invention and the blank sample were tested in a sodium ion battery at 3Ag -1 Long cycle diagram under current density of . DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0034] Example 1

[0035] The preparation method of iodine-doped nano-molybdenum disulfide composite carbon material comprises the following steps:

[0036] (1) Add 1.44 g of glucose to 70 mL of deionized water, add 1.6 g of sodium molybdate dihydrate and 3.2 g of thiourea while stirring, and add 50 mg of sodium iodide after the materials are dissolved.

[0037] (2) After the materials were dissolved, the mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and hydroheated at 200 °C for 24 h.

[0038] (3) After cooling to room temperature, the precursor in the hydrothermal reactor is washed with water or ethanol by high-speed centrifugation until the solution is clear, and then dried at 60°C.

[0039] (4) The dried powder is ground and placed in a crucible, and then transferred to a tubular furnace for heating under nitrogen protection at 500° C. for 2 hours at a heating rate of 5° C. / min. After the heating is completed, the powder is naturally cooled to room temperature and taken out to obtain an iodine-doped nano-molybdenum disulfide composite carbon material.

[0040] Figure 1 This is a transmission electron microscope image of the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 1. Figure 1 It can be seen that after the introduction of iodine doping, 1T phase appears in its crystal structure.

[0041] Example 2

[0042] The preparation method of iodine-doped nano-molybdenum disulfide composite carbon material is different from that of Example 1 in that, in step (2), hydrothermal treatment is performed at 180° C. for 25 h, and the remaining steps are consistent with those of Example 1 to obtain iodine-doped nano-molybdenum disulfide composite carbon material.

[0043] After testing, the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 2 induced iodine ions to 2H-MoS 2 Stable phase transition to 1T-MoS 2 .

[0044] Example 3

[0045] The preparation method of iodine-doped nano-molybdenum disulfide composite carbon material is different from that of Example 1 in that, in step (2), hydrothermal treatment is performed at 220° C. for 20 h, and the remaining steps are consistent with those of Example 1 to obtain iodine-doped nano-molybdenum disulfide composite carbon material.

[0046] After testing, the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 3 induced iodine ions to 2H-MoS 2 Stable phase transition to 1T-MoS 2 .

[0047] Example 4

[0048] The preparation method of iodine-doped nano-molybdenum disulfide composite carbon material is different from that of Example 1 in that, in step (4), the heating temperature is 520°C, 1.5 hours, and the heating rate is 6°C / min. The remaining steps are consistent with Example 1 to obtain iodine-doped nano-molybdenum disulfide composite carbon material.

[0049] After testing, the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 4 induced iodine ions to 2H-MoS 2 Stable phase transition to 1T-MoS 2 .

[0050] Example 5

[0051] The preparation method of iodine-doped nano-molybdenum disulfide composite carbon material is different from that of Example 1 in that, in step (4), heating is performed at 480°C for 2.5 hours with a heating rate of 4°C / min, and the remaining steps are consistent with those of Example 1 to obtain iodine-doped nano-molybdenum disulfide composite carbon material.

[0052] After testing, the iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 5 induced iodine ions to 2H-MoS 2 Stable phase transition to 1T-MoS 2 .

[0053] Example 6

[0054] A method for preparing a sodium ion battery comprises the following steps:

[0055] (1) The iodine-doped nano-molybdenum disulfide composite carbon material prepared in Example 1, CMC and conductive carbon black are mixed uniformly in a mass ratio of 8:1:1, and then dispersed into a deionized water solution to form a uniform slurry; the slurry is then coated on a copper foil and vacuum dried at 90° C. to obtain a molybdenum disulfide electrode sheet, which is used as a negative electrode for a sodium ion battery.

[0056] (2) Pair the molybdenum disulfide electrode obtained in step (1) with a metallic sodium negative electrode, assemble a CR2032 button cell in an inert gas, and test the electrochemical performance of the molybdenum disulfide electrode. The electrolyte is 1M NaPF 6 in DIGLYME=100Vol%. The button cell structure includes a positive electrode shell (stainless steel), a negative electrode shell (stainless steel), a gasket (stainless steel), a spring (stainless steel), a molybdenum disulfide electrode sheet, a sodium sheet, an electrolyte and a diaphragm (glass fiber).

[0057] Comparative Example 1

[0058] The preparation method of blank sample nano molybdenum disulfide composite carbon material comprises the following steps:

[0059] (1) Add 1.44 g of glucose to 70 mL of deionized water, and add 1.6 g of sodium molybdate dihydrate and 3.2 g of thiourea while stirring.

[0060] (2) After the materials were dissolved, the mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and hydroheated at 200 °C for 24 h.

[0061] (3) After cooling to room temperature, the precursor in the hydrothermal reactor is washed with water or ethanol by high-speed centrifugation until the solution is clear, and then dried at 60°C.

[0062] (4) The dried powder is ground and placed in a crucible, and then transferred to a tubular furnace for heating under nitrogen protection at 500°C for 2 hours at a heating rate of 5°C / min. After the heating is completed, it is naturally cooled to room temperature and taken out to obtain a blank sample of nano-molybdenum disulfide composite carbon material.

[0063] After testing, the blank sample nano-molybdenum disulfide composite carbon material prepared in Comparative Example 1 contained 2H-MoS 2 No phase transition to 1T-MoS 2 .

[0064] Comparative Example 2

[0065] A method for preparing a sodium ion battery comprises the following steps:

[0066] (1) The blank sample nano-molybdenum disulfide composite carbon material, CMC and conductive carbon black prepared in Comparative Example 1 were mixed uniformly in a mass ratio of 8:1:1, and then dispersed into a deionized water solution to form a uniform slurry; the slurry was then coated on a copper foil and vacuum dried at 90° C. to obtain a molybdenum disulfide electrode sheet, which was used as a negative electrode for a sodium ion battery.

[0067] (2) Pair the molybdenum disulfide electrode sheet in step (1) with a metallic sodium negative electrode, assemble a CR2032 button cell in an inert gas, and test the electrochemical performance of the molybdenum disulfide electrode sheet. The electrolyte is 1M NaPF 6 in DIGLYME=100Vol%. The button cell structure includes a positive electrode shell (stainless steel), a negative electrode shell (stainless steel), a gasket (stainless steel), a spring (stainless steel), a molybdenum disulfide electrode sheet, a sodium sheet, an electrolyte and a diaphragm (glass fiber).

[0068] Experimental Example 1 Performance Test of Sodium Ion Anode Material

[0069] Taking the button cell assembled in Example 6 as an example, the cycle performance of the battery assembled with iodine-doped nano-molybdenum disulfide composite carbon material was evaluated using a charge and discharge device (Blue Electric CT3002A). At the same time, as a comparison, the above performance of the battery assembled with no iodine-doped nano-molybdenum disulfide composite carbon material (Comparative Example 1 blank sample) (Comparative Example 2) was also tested. The results are as follows: Figure 2 shown.

[0070] Depend on Figure 2 It can be seen that at a current density of 3Ag -1Under the condition of 3Ag, after 1000 cycles, the charge and discharge specific capacity of iodine-doped nano-MoS2 composite carbon material is higher than that of undoped MoS2 electrode. -1 The specific capacity can reach 550 mAh g -1 The specific capacity of the blank sample is 400 mAh g -1 Compared with the blank sample, the rate performance of the iodine-doped MoS2 material has also been improved to a certain extent.

[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An iodine-doped nano-molybdenum disulfide composite carbon material, characterized in that: The invention comprises iodine-doped nano molybdenum disulfide sheets and amorphous carbon. The iodine-doped nano molybdenum disulfide sheets are stacked into a three-dimensional nano flower structure, and the amorphous carbon covers the surface of the iodine-doped nano molybdenum disulfide sheets.

2. The iodine-doped nano-molybdenum disulfide composite carbon material according to claim 1, characterized in that: The nano molybdenum disulfide includes 2H phase molybdenum disulfide and 1T phase molybdenum disulfide.

3. A method for preparing the iodine-doped nano-molybdenum disulfide composite carbon material according to claim 1 or 2, characterized in that: The steps include: At room temperature, a carbon source is dissolved in water, and then a molybdenum source, a sulfur source, and finally an iodine source are added in sequence to obtain a mixed solution; The obtained mixed solution is subjected to a hydrothermal reaction to obtain a precursor material; The obtained precursor material is calcined under a protective atmosphere to obtain an iodine-doped nano-molybdenum disulfide composite carbon material.

4. The preparation method according to claim 3, characterized in that: The carbon source includes glucose, sucrose or citric acid, preferably glucose; Preferably, the molybdenum source comprises sodium molybdate or ammonium molybdate, preferably sodium molybdate; Preferably, the sulfur source comprises thiourea, sodium thioacetate or ammonium sulfate, preferably thiourea; Preferably, the iodine source is sodium iodide.

5. The preparation method according to claim 3, characterized in that: The carbon source is glucose, the molybdenum source is sodium molybdate, the sulfur source is thiourea, and the iodine source is sodium iodate; Preferably, the mass ratio of glucose, sodium molybdate, thiourea and sodium iodide is (0.8-1):1:2:(0.3-0.4), preferably 0.9:1:2:0.3125.

6. The preparation method according to claim 3, characterized in that: The hydrothermal reaction has a reaction temperature of 180-220° C. and a reaction time of 20-25 h.

7. The preparation method according to claim 3, characterized in that: The precursor material is centrifuged with a washing liquid, dried, and then calcined; Preferably, the drying temperature is 50-70°C; Preferably, the calcination has a heating rate of 4-6°C / min, a calcination temperature of 480-520°C, and a calcination time of 1.5-2.5h.

8. The preparation method according to claim 3, characterized in that: The protective atmosphere is a nitrogen atmosphere or an argon atmosphere, preferably a nitrogen atmosphere.

9. A sodium ion battery negative electrode, characterized in that: It includes a current collector, a binder, a conductive agent and a negative electrode active material; The binder, the conductive agent and the negative electrode active material are mixed and attached to at least one surface of the current collector; The negative electrode active material is the iodine-doped nano-molybdenum disulfide composite carbon material as described in claim 1 or 2, or the iodine-doped nano-molybdenum disulfide composite carbon material prepared by the preparation method described in any one of claims 3-8.

10. A sodium ion battery, characterized in that: It comprises a positive electrode and a negative electrode, wherein the negative electrode is the negative electrode of the sodium ion battery according to claim 9.