Catalyst for dimethylnaphthalene isomerization reaction as well as preparation method and application of catalyst
By modifying the combination of zeolite molecular sieve, kaolin and silica sol, combined with acid-modified binder, the problem of poor thermal conductivity and coke growth in the fluidized bed reactor is solved, and the efficiency of dimethylnaphthalene isomerization reaction is improved and product purity.
Patent Information
- Application Number
- CN202310638430.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
When used in fluidized bed reactors, existing catalysts have problems such as poor thermal conductivity, limited gas flow rate by pressure drop, insufficient utilization of catalyst active surface and coking affects stability, making it difficult to effectively carry out dimethyl naphthalene isomerization reaction.
A catalyst composed of 65-85% zeolite molecular sieve, 5-30% support and 5-30% binder contains phosphorus compounds and rare earth compounds. The acid center and acid distribution are improved through phosphorus and rare earth modification, and combined with kaolin In combination with silica sol, an acid modified binder is used to improve the thermal stability and wear strength of the catalyst.
Improves the thermal stability and hydrothermal stability of the catalyst, reduces dry gas and coke yields, enhances the wear strength and bulk density of the catalyst, is suitable for the application of fluidized bed reactors, and improves the isomerization of dimethylnaphthalene Activity and purity of the product.
Smart Images

Figure BDA0004262404670000111 
Figure BDA0004262404670000121 
Figure HDA0004262404680000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalysts, and more particularly to a catalyst for producing 2,6-dimethylnaphthalene by isomerizing hydrocarbon oil rich in dimethylnaphthalene, such as catalytic cracking light cycle oil, in a fluidized bed reactor, and a preparation method thereof, as well as a method for isomerizing dimethylnaphthalene. Background Art
[0002] 2,6-Dimethylnaphthalene (2,6-DMN) is an important organic chemical raw material. Its oxide 2,6-naphthalene dicarboxylic acid reacts with ethylene glycol to produce a new high-performance polyester material polyethylene 2,6-naphthalene dicarboxylate (PEN). PEN has excellent heat resistance, mechanical properties, gas barrier properties, chemical stability and radiation resistance, and has a very broad application prospect.
[0003] Catalytic cracking light cycle oil is rich in dimethylnaphthalene, usually around 20-40%, and has a low cetane number. It is difficult to use it as a diesel blending component in diesel quality upgrading, but it is a potential cheap resource of 2,6-dimethylnaphthalene. Isomerizing its rich dimethylnaphthalene to increase the content of 2,6-DMN, and then separating and purifying it will have good development prospects.
[0004] Heterogeneous phase selective molecular sieves have controllable porous structures, molecular-sized pores, strong thermal and water stability, large specific surface area, a large number of pores and a large number of surface acid sites, and are often used as catalysts for isomerization reactions. Mordenite is often used as an isomerization catalyst. Sinopec patents CN103100413A, CN103041843B and CN103041844B report the preparation method of modified mordenite isomerization catalyst for alkane isomerization, and the catalyst includes a Pt metal component, a rare earth modified molecular sieve and a carrier.
[0005] Sanleng Gas Chemical Company's patents US5495060A and US5481055A reported a method for isomerizing a mixture mainly composed of 1,6-dimethylnaphthalene to produce 2,6-dimethylnaphthalene, using H-type mordenite as a catalyst. If the catalyst is Na-type or Ca, its catalytic activity will be affected. Global Oil Company's patent US4777312A also uses H-type mordenite as a catalyst. Unlike Sanleng Gas Chemical's patent, this method uses Group VIII noble metals to modify the catalyst, and uses H2 as the atmosphere during the reaction. This process is more suitable for the isomerization of other 2,7-dimethylnaphthalene to produce 2,6-dimethylnaphthalene.
[0006] The traditional dimethylnaphthalene isomerization catalyst is a fixed bed reactor catalyst. The fixed bed often has the disadvantages of poor thermal conductivity and too large gas flow rate limitation by pressure drop, resulting in poor heat transfer performance of the bed and difficulty in controlling temperature. In addition, fine-particle catalysts cannot be used during the reaction, and the active surface of the catalyst is not fully utilized. Aromatic hydrocarbon oil will produce coke while reacting on the molecular sieve catalyst, which will affect the operating stability of the device and reduce the activity of the isomerization reaction. The fluidized bed reactor has high volume utilization, short reaction time, large processing capacity, easy regeneration, and is more suitable for long-term continuous operation of large-scale production. Therefore, the art needs to develop a catalyst for the isomerization of dimethylnaphthalene that is particularly suitable for fluidized bed reactors. Summary of the invention
[0007] The present invention aims to solve the problems existing in the existing catalysts, prepare a catalyst for a fluidized bed reactor, and realize the isomerization reaction of dimethylnaphthalene-rich hydrocarbon oil to continuously produce 2,6-dimethylnaphthalene.
[0008] The present application provides a catalyst for the isomerization reaction of dimethylnaphthalene, which comprises the following components based on the mass of the catalyst: 65-85% of a zeolite molecular sieve, 5-30% of a carrier and 5-30% of a binder, wherein the zeolite molecular sieve contains 0.1-2.0wt% of a phosphorus compound calculated as P2O5 and 0.1-2.0wt% of a rare earth compound calculated as RE2O3.
[0009] In one embodiment, the zeolite molecular sieve is mordenite or H-type mordenite.
[0010] In one embodiment, the rare earth is selected from one or more of lanthanum, cerium, neodymium, and praseodymium, preferably lanthanum and cerium.
[0011] In one embodiment, the carrier is clay, selected from one or more of pseudo-boehmite, kaolin, halloysite, montmorillonite, diatomaceous earth, hydrotalcite and bentonite, preferably kaolin or halloysite.
[0012] In one embodiment, the binder may be selected from one or more of silica sol, alumina sol, silica-alumina sol or phospho-alumina sol, preferably silica sol.
[0013] The present application also relates to a method for preparing a catalyst, comprising:
[0014] S1. A zeolite molecular sieve is impregnated with a mixed solution of phosphate and rare earth salt, and then dried and calcined to obtain a modified zeolite molecular sieve;
[0015] S2. The modified zeolite molecular sieve is subjected to ammonium ion exchange, and then calcined in the presence of water vapor to obtain an ultrastable H-type mordenite;
[0016] S3. The ultrastable H-type mordenite and the aged carrier are formed into a catalyst precursor slurry, an acid-modified binder and a pore-forming agent are added to form a catalyst precursor sol, and the catalyst precursor sol is formed and calcined to obtain the catalyst.
[0017] In one embodiment, the phosphate is selected from one or more of neutral phosphate, hydrogen phosphate, and dihydrogen phosphate;
[0018] The rare earth salt is one or more of nitrates, sulfates and chlorides of rare earth.
[0019] In one embodiment, in S1, based on the dry basis of the molecular sieve, the mixed solution contains 0.1-2.0% of phosphorus compounds calculated as P2O5, 0.1-2.0% of rare earth compounds calculated as RE2O3, and the weight ratio of the mixed solution of phosphate and rare earth salt to the zeolite molecular sieve is 1-5:1; the calcination temperature is 400-500°C, and the time is 2-4 hours.
[0020] In one embodiment, in S2, the calcination temperature is 400-600° C. and the calcination time is 2-4 hours.
[0021] In one embodiment, in S3, the aged carrier is prepared as follows: the carrier is dispersed in deionized water to form a slurry, the pH value is adjusted to 2-4, and then allowed to stand for aging;
[0022] The acid-modified binder is prepared as follows: the pH of the binder is adjusted to less than 7 with an acid, wherein the acid is preferably an organic acid, and the organic acid is selected from one or more of citric acid, acetic acid, oxalic acid, and succinic acid, preferably citric acid and acetic acid;
[0023] Before the acid-modified binder is added to the catalyst precursor slurry, deionized water is added for dilution, and the mass ratio of the deionized water to the acid-modified binder is 1-10:1.
[0024] In one embodiment, the pore former is selected from one or more of sesbania powder, methyl cellulose, carboxymethyl cellulose and cellulose acetate.
[0025] In one embodiment, in S3, the calcination temperature is 500-800°C.
[0026] The present application also relates to a method for isomerizing dimethylnaphthalene, comprising: contacting a hydrocarbon oil rich in dimethylnaphthalene with the catalyst of the present application under conditions sufficient for isomerizing the dimethylnaphthalene.
[0027] In one embodiment, the method is carried out in a fluidized bed reactor, and the reaction conditions include: a reaction temperature of 250 to 450° C., a reaction pressure of 0.1 to 0.5 MPa, a residence time of 4 to 12 seconds, and a weight ratio of catalyst to feedstock oil of 1 to 6:1.
[0028] The catalyst of the present application contains phosphorus compounds and rare earth compounds. Rare earth modification helps to improve the acid center of the zeolite molecular sieve, while phosphorus modification helps to adjust the acid distribution of the zeolite molecular sieve, thereby reducing the cracking activity of the catalyst and improving the isomerization activity of dimethylnaphthalene, and is also beneficial to increase the thermal stability and hydrothermal stability of the catalyst. At the same time, in order to further improve the thermal stability and hydrothermal stability of the catalyst, the modified molecular sieve is hydrothermally treated during the preparation process; and, during the preparation process, by using a combination of kaolin and silica sol, the prepared catalyst can have better wear strength and larger bulk density, which is more conducive to the application of the catalyst in a fluidized bed reactor; the use of an acid-modified binder can reduce the dry gas and coke content in oil and gas products, while improving the wear strength of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A system for producing 2,6-dimethylnaphthalene using a fluidized bed reactor is shown. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below through examples. Through these examples, the features and advantages of the present invention will become clearer and more specific.
[0031] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0032] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0033] The present application relates to a catalyst for isomerization reaction of dimethylnaphthalene, which comprises the following components based on the mass of the catalyst: 65-85% of zeolite molecular sieve, 5-30% of carrier and 5-30% of binder, wherein the zeolite molecular sieve contains 0.1-2.0wt% of phosphorus compound calculated as P2O5 and 0.1-2.0wt% of rare earth compound calculated as RE2O3.
[0034] When using hydrocarbon oil rich in dimethylnaphthalene such as catalytic cracking light cycle oil as a raw material for dimethylnaphthalene isomerization reaction, the isomerization catalyst needs to reduce the catalytic ability of the cracking reaction and enhance the catalytic ability of the isomerization reaction according to the raw material properties of the catalytic cracking light cycle oil itself. The catalyst of the present application contains a phosphorus compound and a rare earth compound. Rare earth modification helps to improve the acid center of the zeolite molecular sieve, and phosphorus modification helps to adjust the acid distribution of the zeolite molecular sieve, thereby reducing the cracking activity of the catalyst and improving the isomerization activity of dimethylnaphthalene, and is also conducive to increasing the thermal stability and hydrothermal stability of the catalyst.
[0035] In one embodiment, the zeolite molecular sieve is mordenite or H-type mordenite. In one embodiment, the rare earth is selected from one or more of lanthanum, cerium, neodymium, and praseodymium, preferably lanthanum and cerium.
[0036] In one embodiment, the carrier is clay, selected from one or more of pseudo-boehmite, kaolin, halloysite, montmorillonite, diatomaceous earth, hydrotalcite and bentonite, preferably kaolin or halloysite. In one embodiment, the binder can be selected from one or more of silica sol, alumina sol, silica-alumina sol or phosphoalumina sol, preferably silica sol.
[0037] When the isomerization raw material is a hydrocarbon oil rich in dimethylnaphthalene, such as catalytic cracking light cycle oil, the hydrocarbon oil is prone to cracking reaction to produce dry gas and coke. In addition, the existing dimethylnaphthalene isomerization catalyst is mainly composed of precious metals, molecular sieves and alumina carriers, and the mass proportion of molecular sieves is more than 60%. The alumina carrier with a small proportion is difficult to provide the catalyst strength and hydrothermal stability required for the fluidized bed reactor reaction. During the research process, the inventors of this application found that the carrier obtained by combining kaolin as a carrier and silica sol as a binder has a lower cracking activity, making the mordenite molecular sieve catalyst more conducive to the isomerization reaction, and less coke and dry gas are produced. It was also found that the catalyst prepared by kaolin and silica sol has better wear strength and larger bulk density, which is more conducive to the application of the catalyst in a fluidized bed reactor. However, in the process of using silica sol to prepare the catalyst, the silica sol easily reacts with aluminum ions to form a precipitate and becomes a gel. The gel carrier has a strong cracking performance, which leads to an increase in the dry gas and coke content in the oil and gas products when the catalyst is used for isomerization reaction. At the same time, the gel will also reduce the wear strength of the catalyst. The inventors of the present application have found that the use of acid-modified binders and adding them after dilution can overcome this problem. The modification conditions are: adding an organic acid solution to the binder sol, especially the silica sol, so that the acid solution and the silica sol are evenly stirred to form a colloid with a pH less than 7.
[0038] Therefore, the present application provides a method for preparing the catalyst of the present application, comprising:
[0039] S1. A zeolite molecular sieve is impregnated with a mixed solution of phosphate and rare earth salt, and then dried and calcined to obtain a modified zeolite molecular sieve;
[0040] S2. The modified zeolite molecular sieve is subjected to ammonium ion exchange, and then calcined in the presence of water vapor to obtain an ultrastable H-type mordenite;
[0041] S3. The ultrastable H-type mordenite and the aged carrier are formed into a catalyst precursor slurry, an acid-modified binder and a pore-forming agent are added to form a catalyst precursor sol, and the catalyst precursor sol is formed and calcined to obtain the catalyst.
[0042] Step S1 is the phosphorus and rare earth modification of zeolite molecular sieve. A mixed solution of phosphate and rare earth salt can be prepared using deionized water, and then the zeolite molecular sieve is impregnated at 70-80°C, dried at 50-120°C, and roasted at 400-500°C for 2-4h. The phosphate is selected from one or more of neutral phosphates, hydrogen phosphates, and dihydrogen phosphates; for example, phosphates, hydrogen phosphates, and dihydrogen phosphates of alkali metals such as sodium and potassium, phosphates, hydrogen phosphates, and dihydrogen phosphates of ammonium ions. The rare earth salt is one or more of rare earth nitrates, sulfates, and chlorides, such as lanthanum nitrate, cerium nitrate, and the like.
[0043] In one embodiment, in S1, based on the molecular sieve dry basis, the mixed solution contains 0.1-2.0% of phosphorus compound calculated as P2O5, 0.1-2.0% of rare earth compound calculated as RE2O3, and the weight ratio of the mixed solution of phosphate and rare earth salt to the zeolite molecular sieve is 1-5: 1. In S1, when the zeolite molecular sieve is impregnated with the mixed solution of phosphate and rare earth salt, an equal volume impregnation or an excess impregnation method is adopted.
[0044] In one embodiment, in S1, the calcination temperature is 400-500° C. and the calcination time is 2-4 hours.
[0045] Step S2 is a hydrothermal modification step of the zeolite molecular sieve. The zeolite molecular sieve modified by phosphorus and rare earth can be subjected to ammonium ion exchange, for example, mixed with an ammonium ion solution such as a 2-4 wt% ammonium chloride aqueous solution, and then subjected to ion exchange in a reactor at a temperature of 70-80°C. The zeolite molecular sieve after ammonium ion exchange is then calcined at 400-600°C for 2-4h, and water vapor is introduced during the calcination process to obtain an ultra-stable H-type mordenite.
[0046] Step S3 is a catalyst forming step. The ultrastable H-type mordenite and the aged carrier are formed into a catalyst precursor slurry, an acid-modified binder and a pore-forming agent are added to form a catalyst precursor sol, and the catalyst precursor sol is formed and calcined to obtain the catalyst. This can be done as follows:
[0047] Use deionized water to slurry the carrier, add acid to adjust the pH to 2-4, and then let it stand for aging. Ultra-stable H-type mordenite and deionized water are slurried at a solid-liquid ratio of 1:1-1:10 and added to the carrier slurry, and an acid-modified binder and pore-forming agent are added. The mixture is placed in a mixer until a uniform sol is formed and sprayed into shape.
[0048] In S3, the acid-modified binder is prepared as follows: the pH of the binder is adjusted to less than 7 with an acid, wherein the acid is preferably an organic acid, and the organic acid is selected from one or more of citric acid, acetic acid, oxalic acid, and succinic acid, preferably citric acid and acetic acid;
[0049] Before the acid-modified binder is added to the catalyst precursor slurry, deionized water is also added, and the mass ratio of the deionized water to the acid-modified binder is 1-10:1.
[0050] In one embodiment, the pore former is selected from one or more of sesbania powder, methyl cellulose, carboxymethyl cellulose and cellulose acetate.
[0051] In one embodiment, in S3, the calcination temperature is 500-800°C.
[0052] The catalyst used in the fluidized bed reactor is generally in the form of microspheres, with a diameter of 20 to 200 microns, preferably 40 to 150 microns. The catalyst of the present invention needs to be hydrothermally treated at 500 to 600° C. for 4 to 8 hours under steam before use to reduce the initial activity.
[0053] The catalyst of the present application can be used for isomerization of dimethylnaphthalene to prepare 2,6-dimethylnaphthalene. Therefore, the present application also relates to a method for isomerization of dimethylnaphthalene, comprising: contacting a hydrocarbon oil rich in dimethylnaphthalene with the catalyst of the present application under conditions sufficient for isomerization of dimethylnaphthalene. In one embodiment, the isomerization process is carried out in a fluidized bed reactor, and the reaction conditions include: a reaction temperature of 250 to 450°C, a reaction pressure of 0.1 to 0.5 MPa, a residence time of 4 to 12 seconds, and a catalyst to feedstock oil weight ratio of 1 to 6:1. In particular, the catalyst of the present application still has a very high isomerization activity at a lower temperature, such as 250 to 350°C, and can be used for isomerization reaction at a lower reaction temperature, which can save energy.
[0054] The catalyst can be regenerated after being deactivated by coking. The regeneration conditions are: temperature of 450-560°C, pressure of 1-1.0MPa, and atmosphere of oxygen-containing gas.
[0055] The raw materials used in the above-mentioned dimethylnaphthalene isomerization method are a dimethylnaphthalene mixture and a hydrocarbon oil rich in dimethylnaphthalene, wherein the hydrocarbon oil includes but is not limited to catalytic cracking light cycle oil, coal tar, ethylene tar and / or other dimethylnaphthalene-rich fractions from other devices, wherein the content of dimethylnaphthalene is 10-80% by weight, for example, 10-50% by weight.
[0056] In one embodiment, the method for isomerizing dimethylnaphthalene can be carried out Figure 1 The fluidized bed reactor is used in the system for producing 2,6-dimethylnaphthalene, and the system comprises:
[0057] Fluidized bed reactor,
[0058] Separation system,
[0059] a catalyst regenerator 14, and
[0060] Catalyst degassing device 18;
[0061] The fluidized bed reactor comprises an inlet section I, a reaction section II, a separation section III and an outlet section IV;
[0062] The inlet section I is provided with a catalyst feed port I-1 and a dimethylnaphthalene feed oil feed port I-2; the oil and gas outlet of the outlet section IV is connected to the oil and gas inlet of the separation system, and the separation system is provided with a 2,6-dimethylnaphthalene outlet 12;
[0063] The separation section III includes a transition section III-1, a stripping section III-2 and a separator III-3; the transition section III-1 is connected between the outlet of the reaction section II and the inlet of the separator III-3;
[0064] The oil and gas outlet of the separator III-3 is connected to the oil and gas inlet of the outlet section IV, the catalyst outlet of the separator III-3 is connected to the catalyst inlet of the stripping section III-2, the catalyst outlet of the stripping section III-2 is connected to the catalyst inlet to be regenerated of the catalyst regenerator 14, and the oil and gas outlet of the stripping section III-2 is connected to the oil and gas inlet of the outlet section IV;
[0065] The regenerated catalyst outlet of the catalyst regenerator 14 is connected to the catalyst inlet of the catalyst degassing device 18, and the catalyst outlet of the catalyst degassing device 18 is connected to the catalyst feed port I-1 of the inlet section I;
[0066] The inner diameter ratio of the reaction section II to the inlet section I is 2-10:1, preferably 2-5:1, and the inner diameter ratio of the reaction section II to the transition section III-1 is 2-10:1, preferably 2-5:1.
[0067] It should be noted that in the system described in the present invention, the dimethylnaphthalene feedstock oil 1 enters the inlet section I through the dimethylnaphthalene feedstock oil feed port I-2, and the fluidized bed reactor adopts a bottom feeding method. Under the fluidization of the fluidized medium 2, the dimethylnaphthalene feedstock oil 1 contacts the isomerization catalyst in the reaction section II for isomerization reaction. The oil mixture obtained in the reaction section II enters the separator III-3 through the transition section III-1 for separation to obtain the separation catalyst and the first oil-gas mixture. The first oil-gas mixture enters the outlet section IV, and the separation catalyst enters the stripping section III-2 to separate the oil, gas, hydrogen, light hydrocarbons and other flammable gases remaining or entrained on the separation catalyst by nitrogen and / or water vapor stripping to obtain the catalyst to be regenerated and the second oil-gas mixture. The stripped catalyst to be regenerated enters the catalyst regenerator 14 for regeneration, and the regenerated catalyst enters the inlet section I through the catalyst feed port I-1 after being degassed by the catalyst degassing device 18, and the second oil-gas mixture obtained by stripping enters the outlet section IV. The first oil-gas mixture separated by the separator III-3 and the second oil-gas mixture obtained by stripping in the stripping section III-2 can be filtered by a filtering device and then enter the separation system for separation to obtain the target product 2,6-dimethylnaphthalene.
[0068] It should be noted that the separation section III can be a rapid separation section. The inner diameter of the reactor from the inlet section I to the reaction section II becomes larger, and the residence time becomes longer, which is conducive to better progress of the isomerization reaction; the inner diameter of the reactor from the reaction section II to the transition section III-1 becomes smaller, the apparent linear velocity of oil and gas increases, and the residence time becomes shorter, which is conducive to the rapid separation of hydrocarbon oil and catalyst after the reaction. Therefore, the system can prepare 2,6-dimethylnaphthalene more efficiently.
[0069] According to a specific embodiment of the system of the second aspect of the present invention, the separation system comprises an oil-gas separation system 5 and a separation and purification system 11; the oil-gas outlet of the outlet section IV is connected to the oil-gas inlet of the oil-gas separation system 5;
[0070] The oil-gas separation system 5 is provided with a dry gas outlet 6, a liquefied gas outlet 7, a gasoline outlet 8, a diesel outlet 9 and a circulating oil outlet 10; the diesel outlet 9 is connected to the inlet of the separation and purification system 11, and the separation and purification system 11 is provided with a residual diesel outlet 13 and the 2,6-dimethylnaphthalene outlet 12;
[0071] The inlet section I is provided with a recycled oil inlet I-3, and the remaining diesel outlet 13 and the circulating oil outlet 10 are respectively connected to the recycled oil inlet I-3.
[0072] It should be noted that the oil-gas separation system 5 can be specifically a fractionation tower, an absorption-stabilization system, etc., and the separation and purification system 11 can be specifically a distillation tower, an extraction tower, a washing tower, a crystallization tower, etc. The regenerative thermal catalyst contacts the feedstock oil and the circulating oil under hydrogen and / or nitrogen fluidization, and enters the inlet section and the reaction section from the lower part of the fluidized bed reactor in sequence for isomerization reaction. The oil-gas mixture obtained by the separator III-3 and the stripping section III-2 enters the outlet section IV, and the oil-gas mixture enters the oil-gas separation system 5 through the outlet section IV. After the separation process of the oil-gas separation system 5, dry gas, liquefied gas, gasoline, diesel and circulating oil are obtained. The diesel enters the separation and purification system 11, and 2,6-dimethylnaphthalene and residual diesel are obtained after separation and purification. The residual diesel and circulating oil enter the inlet section I through the refining oil inlet I-3, and contact with the isomerization catalyst for isomerization reaction.
[0073] In one embodiment, a filter IV-1 is provided between the oil and gas outlet of the outlet section IV and the oil and gas inlet of the oil and gas separation system 5; and / or,
[0074] The oil and gas outlet of the outlet section IV is connected to the oil and gas inlet of the oil and gas separation system 5 through an oil and gas pipeline 4; and / or,
[0075] The stripping section III-2 is provided with a stripping medium inlet 3, and the catalyst outlet of the stripping section III-2 is connected to the catalyst inlet to be regenerated of the catalyst regenerator 14 through a regeneration pipeline 19; and / or,
[0076] The regenerated catalyst outlet of the catalyst regenerator 14 is connected to the catalyst inlet of the catalyst degassing device 18 via a regeneration pipeline 17; and / or,
[0077] The catalyst regenerator 14 is provided with an oxygen-containing gas inlet 15 and a flue gas outlet 16;
[0078] And / or, the fluidized bed reactor is selected from a combination of one or more of a bubbling bed, a turbulent bed, a fast bed and a transport bed;
[0079] When the fluidized bed reactor is a combination of multiple types, the combination of the multiple fluidized bed reactors is in series and / or parallel connection; and / or,
[0080] The catalyst degassing device 18 is a degassing tank and / or a stripping device; and / or,
[0081] The fluidized bed reactor and the catalyst regenerator 14 are arranged in parallel or coaxially; and / or,
[0082] The apparent average linear velocity of oil and gas in the reaction section II is 0.5 to 3 m / s.
[0083] The following examples will further illustrate the method, but do not limit the method. The mordenite used in the examples was purchased from Yingkou Zhongbao Molecular Sieve Co., Ltd.
[0084] Example 1
[0085] The catalyst in Example 1 was synthesized according to the following steps:
[0086] 1) With 1.0 kg of mordenite molecular sieve as the matrix, 1.0 kg of deionized water is used to prepare a mixed solution of 5 g of ammonium dihydrogen phosphate as P2O5, 10 g of lanthanum nitrate as La2O3 and 16 g of cerium nitrate as CeO2, the molecular sieve is impregnated at 70-80°C for 4-8 h, dried at 50-120°C, and calcined at 400-500°C for 2-4 h.
[0087] 2) Use deionized water to prepare an ammonium chloride solution with a concentration of 3% by weight, and then stir the molecular sieve powder that has not been ion-exchanged in a reactor at 70-80°C for 2 hours. After the solution cools down, remove the liquid and wash with deionized water. Repeat 2-3 times to obtain an ammonium-exchanged molecular sieve. The molecular sieve is dried at 120°C and calcined at 500°C for 3 hours. During the calcination, 30mL / min of water vapor is introduced to obtain an ultra-stable H-type mordenite molecular sieve.
[0088] 3) 0.25 kg of kaolin is selected as the carrier and added to deionized water for slurrying to obtain a slurry with a certain solid content. Then, hydrochloric acid is used to adjust the pH to 2-4, and after stirring evenly, it is allowed to stand at about 70°C for a period of time to age it to form a slurry. The H-type molecular sieve obtained in step 2) is added to deionized water for slurrying at a liquid-to-solid ratio of 3.0, and then added to the above slurry, and stirred evenly in a bonding machine to obtain a mixed slurry.
[0089] 4) Using citric acid, adjust the pH of 0.35 kg of silica sol to 4-5, add deionized water at a mass ratio of 5:1 to dilute, and then slowly add to the mixed slurry obtained in step 3), continue to stir evenly, and add 10-20 g of sesbania powder during the stirring process.
[0090] 5) Stop stirring and place for aging for a period of time. Use the spray molding method to shape the obtained sol to obtain a microspherical catalyst, control the tail gas temperature at 250-300°C, and the spray pressure at 50-60 atmospheres. Dry the catalyst at about 120°C for 3 hours, and calcine it at 500°C in a muffle furnace for 3 hours to obtain the catalyst. The catalyst is recorded as CAT-1.
[0091] Comparative Example 1
[0092] The preparation steps 1), 2), 3) and 5) of the catalyst in Comparative Example 1 are the same as those in Example 1, except that in step 4), 0.35 kg of silica sol is slowly added to the mixed slurry obtained in step 3, and stirring is continued to be uniform. During the stirring process, 10 to 20 g of sesbania powder is added. The prepared catalyst is recorded as CAT-2.
[0093] Comparative Example 2
[0094] The preparation steps 2), 3), 4) and 5) of the catalyst of Comparative Example 2 are the same as those of Comparative Example 1, except that there is no phosphorus and rare earth modification in step 1. The prepared catalyst is recorded as CAT-3.
[0095] Table 1
[0096] CAT-1 CAT-2 CAT-3 <![CDATA[Na2O, wt%]]> 0.07 0.01 0.02 <![CDATA[Al2O3, wt%]]> 29.00 30.70 31.80 <![CDATA[SiO2, wt%]]> 68.00 67.60 67.20 <![CDATA[P2O5, wt%]]> 0.25 0.28 0.00 <![CDATA[La2O3, wt%]]> 0.46 0.48 0.00 <![CDATA[CeO2, wt%]]> 0.76 0.70 0.00
[0097] Test Case
[0098] Dimethylnaphthalene isomerization experiment Figure 1 The system shown (including a fluidized bed reactor) is carried out, and the raw oil and recycled oil enter from the bottom of the reactor to contact with the hot catalyst for isomerization reaction, and then the oil agent is separated. The oil and gas generated after the reaction are separated to obtain gas products (dry gas and liquefied gas), gasoline, diesel, and circulating oil. The diesel is further separated to obtain the product 2,6-dimethylnaphthalene, and the remaining diesel and circulating oil are recycled. The catalyst after the reaction is stripped and enters the regenerator for regeneration in the oxygen-containing gas, and the regenerated catalyst is recycled. In this test example, the inner diameter ratio of the reaction section II and the inlet section I of the fluidized bed reactor is 3:1, and the length ratio is 3:1; the inner diameter ratio of the reaction section II and the transition section III-1 is 3:1, and the length ratio is 1:1. Isomerization reaction conditions: reaction temperature is 275℃, agent-oil weight ratio is 3.0, and residence time is 6.2 seconds. The regeneration temperature is 500-560℃. The isomerization reaction results are shown in Table 2.
[0099] The raw oil used was catalytic cracking light cycle oil (properties are shown in Table 2), wherein the content of dimethylnaphthalene was 21.2% by weight and the content of 2,6-dimethylnaphthalene was 3.4% by weight. The catalyst used in Example 2 was CAT-1, and the catalysts used in Comparative Examples 3 and 4 were CAT-2 and CAT-3, respectively. The results are listed in Table 3.
[0100] Table 2
[0101] Basic properties Hydrocarbon composition / wt.% <![CDATA[Density (20 °C) / (g / cm 3 )]]> 0.9954 Total saturated hydrocarbons 1.6 Sulfur content / (μg / g) 14.3 Total aromatics 98.4 Nitrogen content / (μg / g) 1.9 Total monocyclic aromatic hydrocarbons 16.9 Carbon content / % 92.14 Total bicyclic aromatic hydrocarbons 75.3 Water content / (mg / L) 168 Dimethylnaphthalene 21.2 Oxygen content / (mg / L) 384 2,6-Dimethylnaphthalene 3.4 Chlorine content / (mg / kg) 3.1 Total tricyclic aromatic hydrocarbons 6.2 Bromine value / (gBr / 100mL) 2.7 gross weight 100
[0102] Table 3
[0103]
[0104]
[0105] Compared with Example 2, the silica sol used in Comparative Example 3 was not acid-modified and diluted during preparation, resulting in the formation of a gel carrier, so that the resulting comparative catalyst CAT-2 has a certain cracking ability, and the dry gas + coke yield is increased by 1.49 units; at the same time, the gel will seal part of the mordenite in the pores, reducing the isomerization ability of the catalyst, resulting in a 0.35 unit decrease in 2.6-DMN.
[0106] Compared with Example 2, the dry gas + coke yield of Comparative Example 4 is 1.83 percentage points higher, and 2,6-DMN is 0.99 percentage points lower, indicating that the catalyst prepared by using rare earth and phosphorus modified molecular sieves, kaolin carrier and acid-modified silica sol binder is beneficial to reducing dry gas and coke and increasing the isomerization reaction of dimethylnaphthalene.
[0107] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.
Claims
1. A catalyst for isomerization of dimethylnaphthalene, comprising the following components based on the mass of the catalyst: 65-85% of a zeolite molecular sieve, 5-30% of a carrier and 5-30% of a binder, wherein: The zeolite molecular sieve contains 0.1-2.0 wt% of phosphorus compounds calculated as P2O5 and 0.1-2.0 wt% of rare earth compounds calculated as RE2O3.
2. The catalyst according to claim 1, wherein The zeolite molecular sieve is mordenite or H-type mordenite.
3. The catalyst according to claim 1, wherein The rare earth is selected from one or more of lanthanum, cerium, neodymium and praseodymium, preferably lanthanum and cerium.
4. The catalyst according to claim 1, wherein The carrier is clay, selected from one or more of pseudo-boehmite, kaolin, halloysite, montmorillonite, diatomaceous earth, hydrotalcite and bentonite, preferably kaolin or halloysite.
5. The catalyst according to claim 1, wherein The binder can be selected from one or more of silica sol, alumina sol, silica-alumina sol or phospho-alumina sol, preferably silica sol.
6. A method for preparing a catalyst according to any one of claims 1 to 5, comprising: S1. The zeolite molecular sieve is impregnated with a mixed solution of phosphate and rare earth salt, and then dried and calcined to obtain a modified zeolite molecular sieve; S2. The modified zeolite molecular sieve is subjected to ammonium ion exchange, and then calcined in the presence of water vapor to obtain an ultrastable H-type mordenite; S3. The ultrastable H-type mordenite and the aged carrier are formed into a catalyst precursor slurry, an acid-modified binder and a pore-forming agent are added to form a catalyst precursor sol, and the catalyst precursor sol is formed and calcined to obtain the catalyst.
7. The preparation method according to claim 6, wherein: The phosphate is selected from one or more of neutral phosphate, hydrogen phosphate, and dihydrogen phosphate; The rare earth salt is one or more of nitrates, sulfates and chlorides of rare earth.
8. The preparation method according to claim 6, wherein: In S1, based on the dry basis of the molecular sieve, the mixed solution contains 0.1-2.0% of phosphorus compounds calculated as P2O5, 0.1-2.0% of rare earth compounds calculated as RE2O3, and the weight ratio of the mixed solution of phosphate and rare earth salt to the zeolite molecular sieve is 1-5:1; the calcination temperature is 400-500°C, and the time is 2-4 hours.
9. The preparation method according to claim 6, wherein: In S2, the calcination temperature is 400-600°C and the calcination time is 2-4 hours.
10. The preparation method according to claim 6, wherein: In S3, the aged support is prepared as follows: the support is dispersed in deionized water to form a slurry, the pH value is adjusted to 2-4, and then allowed to stand for aging; The acid-modified binder is prepared as follows: the pH of the binder is adjusted to less than 7 with an acid, wherein the acid is preferably an organic acid, and the organic acid is selected from one or more of citric acid, acetic acid, oxalic acid, and succinic acid, preferably citric acid and acetic acid; Before the acid-modified binder is added to the catalyst precursor slurry, deionized water is added for dilution, and the mass ratio of the deionized water to the acid-modified binder is 1-10:
1.
11. The preparation method according to claim 6, wherein: The pore-forming agent is selected from one or more of sesbania powder, methyl cellulose, carboxymethyl cellulose and cellulose acetate.
12. The preparation method according to claim 6, wherein: In S3, the calcination temperature is 500 to 800°C.
13. A method for isomerizing dimethylnaphthalene, comprising: A hydrocarbon oil rich in dimethylnaphthalene is contacted with the catalyst according to any one of claims 1 to 5 or the catalyst obtained by the preparation method according to any one of claims 6 to 12 under conditions sufficient to carry out the isomerization reaction of dimethylnaphthalene.
14. The method according to claim 13, wherein: The method is carried out in a fluidized bed reactor, and the reaction conditions include: reaction temperature of 250-450° C., reaction pressure of 0.1-0.5 MPa, residence time of 4-12 seconds, and a weight ratio of catalyst to crude oil of 1-6:1.