Device and method for preparing 1-10 [mu] m spherical core-shell structure metal powder

Through plasma arc-nano powder growth-plasma arc composite technology, the problems of uneven insulation coating and oxidation risks in the prior art were solved, and 1-10μm spherical core-shell structure metal powder with narrow particle size and high spherical shape were prepared. Improves the performance stability and loss reduction effect of the inductor.

CN119057071AInactive Publication Date: 2024-12-03DONGYANG CHUANGXIAN NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411247045.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, when preparing 1-10 μm spherical core-shell structure metal powder, there are problems such as uneven insulation coating, irregular shape, oxidation risk and low spherical powder, resulting in high loss of integrated molding inductor and unstable performance.

Method used

Using nano powder generation, microparticle growth and core-shell structure generation devices, micron-scale spherical powder with insulated shells is prepared through plasma arc-nano powder growth-plasma arc composite technology, and the collision probability is regulated to control particle size and spherical degree to form 1-10μm spherical core-shell structure metal powder.

Benefits of technology

The core-shell structure preparation of the powder is achieved. The shell is a nanoscale thick oxide, with a narrow particle size distribution and a spherical degree of ≥95%, which reduces eddy current loss and improves the anti-saturation and performance stability of the powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057071A_ABST
    Figure CN119057071A_ABST
Patent Text Reader

Abstract

The invention discloses a device and method for preparing 1-10 [mu] m spherical core-shell structure metal powder, and the device comprises a nanopowder generation device which comprises an arc chamber, a first feeding device, a first vacuum system, a gas path, a cooling system and a gas injection system; the micron particle growing device comprises a forming pipe, a first heating system, a first heat preservation system, a pneumatic system, a slow cooling pipe and a second heating system, the core-shell structure generating device comprises a core-shell forming chamber, a second feeding device and a second heat preservation system; and the passivation insulation collecting device comprises a collecting chamber, a second vacuum system and a passivation gas path. Two processes of preparing 1-10 [mu] m spherical metal powder and insulating coating are combined into one, firstly, high-melting-point metal is made into nanoscale powder, the nanoscale powder is heated to be in a molten state, melt clusters are formed, the melt clusters fall under the action of gravity when the needed size is reached, micron-sized molten spheres are formed under the action of surface tension, cooling is conducted, and micron-sized spherical powder is obtained; and then low-melting-point metal is adsorbed on the surface of the spherical powder under the action of surface adsorption force, and finally passivation is performed to react with oxygen to generate an oxide layer, so that the spherical core-shell structure metal powder of 1-10 microns is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powder preparation, and in particular to a device and method for preparing 1-10 μm spherical core-shell structure metal powder. Background Art

[0002] With the rapid development of the third-generation semiconductor technology, the switching frequency is getting higher and higher, which promotes the "miniaturization, integration, and high frequency" of power devices, which puts higher requirements on the stable power supply and filtering of power inductors. With its advantages in MHz electromagnetic performance, reliability and current resistance, the one-piece molded inductor has become the mainstream of the MHz market. One-piece molded inductors are generally prepared with soft magnetic metal powder. Soft magnetic metal powder, mainly including single soft magnetic metal powder and alloy powder, is the basic electromagnetic functional material of one-piece molded inductors. With the further increase of the operating frequency in the MHz range, the total loss of the one-piece molded inductor will increase significantly, resulting in a rapid increase in the temperature of the one-piece inductor, affecting the working efficiency and performance stability of the one-piece inductor, and even causing the one-piece inductor to fail. Among them, the eddy current loss is proportional to the square of the frequency and occupies the main part of the total loss. There are two main ways to reduce the eddy current loss. One is to increase the resistance of the metal powder and reduce the eddy current in the particles by changing the composition or size of the metal powder; the other is to insulate the metal powder to form a complete core-shell structure to isolate the eddy current between particles. The sphericity and size of the metal powder are important factors affecting its performance and application value. The higher the sphericity and the more regular the particle shape, the stronger the anti-saturation property of the one-piece molded inductor. The resistance of metal powder increases rapidly as the powder particle size decreases, which is beneficial to reduce the eddy current loss inside the powder in the MHz range. However, the smaller the powder particle size, the poorer the fluidity, which affects the performance uniformity of the one-piece molded inductor. Considering the above factors, spherical metal powders of 1 to 10 μm are strong candidate electromagnetic materials for one-piece inductors used in tens of MHz.

[0003] Insulation coating of metal powder is an important process to reduce eddy current loss between particles. Insulating materials are coated on the surface of metal powder to block eddy current between powders and reduce total loss. At present, the insulation coating process of metal powder is to carry out subsequent insulation coating treatment after obtaining the metal powder. The existing subsequent insulation coating treatment is carried out in solution, which will lead to disadvantages such as uneven thickness, irregular shape, and insufficient coating of the insulation coating layer, and it is difficult to play a role in suppressing eddy current loss between particles. In addition, this separate processing process not only increases the complexity of the production process, but also the transfer between processes involves the increase of the total process time and the replacement of different equipment, which undoubtedly leads to the oxidation of 1-10μm metal powder. Therefore, the quality stability of the obtained powder is low, and the heat generated by oxidation poses the risk of heating and fire.

[0004] Spray pyrolysis is one of the few methods that can simultaneously carry out the manufacturing process of soft magnetic powder and the process of insulating soft magnetic powder. The Chinese patent literature discloses "an in-situ oxide layer coated micro-nano rare earth alloy and its preparation method", and its application number is 202411226415.1. The invention patent application discloses that water-soluble samarium salt, water-soluble transition metal salt, SiO2 donor, soluble, high temperature reducing substance or high temperature decomposition to produce reducing substances are mixed and dissolved in water to form a spray precursor solution, and then the ultrasonic spray pyrolysis method is used, and then the calcium reduction diffusion nucleus in-situ chemical reaction is used to obtain a samarium metal alloy coated with calcium silicate with a size of 0.1 to 6 μm. "Insulation coated soft magnetic powder" is disclosed in Chinese patent literature, and its application number is 202280038044.6. This invention patent application discloses that a water-soluble transition metal salt, a SiO2 donor, a soluble substance that has reducing properties at high temperature or produces reducing substances after high-temperature decomposition is made into a raw material solution, and the raw material solution is spray-dried to obtain a mixed oxide powder, which is further crushed by an air flow mill, and then the refined raw material powder is sprayed into a reactor through a carrier gas and a reducing agent for heating treatment. After cooling, an insulation coated soft magnetic powder is obtained. However, when the insulation coated soft magnetic powder is prepared by the spray thermal decomposition method using a liquid raw material, the soft magnetic powder easily reacts with the oxygen from the raw material solution, causing oxidation inside and on the surface of the powder, reducing the magnetic properties of the insulation coated soft magnetic powder. In addition, the alloy powder prepared by this method has poor sphericity and uncontrollable particle size distribution, which weakens the anti-saturation property of the metal powder.

[0005] Therefore, it is urgent to carry out research on a device that integrates powder making and coating processes to produce 1-10μm spherical core-shell structured metal powders. Summary of the invention

[0006] The object of the present invention is to provide a device and method for preparing 1-10μm spherical core-shell structured metal powder. The metal powder prepared by the device has a core-shell structure, the shell is a nano-scale thick oxide, the metal powder particle size is 1-10μm, the particle size distribution is narrow, and the sphericity is ≥95%.

[0007] The present invention is achieved through the following technical solutions.

[0008] The present invention provides a 1-10 μm spherical core-shell structure metal powder preparation device, comprising:

[0009] A nano powder generating device, comprising an arc chamber and a first feeding device connected to the arc chamber, a first vacuum system, a gas path, a cooling system and an injection system, wherein a first electrode is disposed inside the arc chamber;

[0010] A micron particle growth device, the micron particle growth device comprises a forming tube, a first heating system, a first heat preservation system, a pneumatic system, a slow cooling tube and a second heating system, the forming tube is vertically arranged, and has a feed port and a discharge port, the feed port is at the top, the discharge port is at the bottom, the feed port is connected with the arc chamber, the first heating system and the first heat preservation system are arranged outside the forming tube, the pneumatic system is connected with the forming tube to spray gas at a certain pressure into the forming tube and the gas direction is upward, the discharge port is connected with the slow cooling tube, and the second heating system is arranged outside the slow cooling tube;

[0011] A core-shell structure generating device, the core-shell structure generating device comprising a core-shell forming chamber and a second feeding device and a second heat preservation system connected to the core-shell forming chamber, a second electrode is arranged in the core-shell forming chamber, and the core-shell forming chamber is connected to a slow cooling pipe;

[0012] The passivation insulating collection device comprises a collection chamber and a second vacuum system and a passivation gas path connected to the collection chamber, and the collection chamber is communicated with the core-shell molding chamber.

[0013] Furthermore, the first feeding device includes at least one feeding pipe, which is horizontally arranged, and the feeding port of the feeding pipe is located 3 to 5 mm directly below the first electrode; when multiple feeding pipes are provided, the feeding pipes are evenly arranged in concentric circles, and the circular area formed with the center of the circle is the discharge area, the first electrode is located directly above the discharge area, and the diameter of the discharge area is 3 to 5 mm.

[0014] Furthermore, the diameter of the forming tube is not less than 60 mm, and the length is not less than 1 meter. The forming tube is located directly below the feeding port, and the first electrode, the feeding port, and the forming tube are on the same axis.

[0015] Furthermore, the jet system comprises at least one jet pipe, which forms an angle of 45° to 90° with the horizontal line.

[0016] Furthermore, the forming tube has an air inlet, which is located between the feed port and the discharge port, and the pneumatic system is connected to the air inlet, which is located at a position 1 / 2 to 2 / 3 downward of the forming tube.

[0017] Furthermore, the pneumatic system comprises at least one air delivery pipe, and the angle formed downwardly by the air delivery pipe and the axis of the forming pipe is 0° to 45°.

[0018] Furthermore, the second feeding device comprises at least one feeding pipe, the feeding pipe is arranged horizontally, and the discharge port of the feeding pipe is located 3 to 5 mm directly below the second electrode.

[0019] Furthermore, a delivery pipe connected to the slow cooling pipe is provided in the core-shell molding chamber, the delivery pipe changes in diameter and gradually shrinks from top to bottom, and the second electrode is arranged close to the delivery pipe.

[0020] The present invention also provides a method for preparing 1-10 μm spherical core-shell structure metal powder, which is prepared by using the above-mentioned preparation device, comprising the following steps:

[0021] Step 1: The nano powder generating device converts the high melting point metal raw material into nano metal powder, and blows the nano metal powder into the forming tube through the jet system;

[0022] Step 2: The first heating system heats the nano-scale metal powder into a molten state, and the pneumatic system sprays gas at a certain pressure into the forming tube to provide an upward supporting force. The molten metal powder collides and grows into melt clusters until the gravity reaches the required size greater than the supporting force and falls into the slow cooling tube. During the falling process, micron-scale spherical metal powder is formed under the action of surface tension. The micron-scale spherical metal powder is then heated by the second heating system to a surface temperature less than the melting point of the inner core metal and greater than the melting point of the outer shell metal, and enters the core-shell forming chamber;

[0023] Step 3: The low melting point metal raw material is made into metal gas, whose melting point is lower than that of the high melting point metal. Under the surface adsorption force of the micron-sized spherical metal powder, the metal gas is adsorbed on the surface and melted to form micron particles with core-shell structure;

[0024] Step 4: The core-shell structured micron particles enter the collection chamber, and a gas containing oxygen is introduced into the passivation gas path, eventually forming a 1-10 μm spherical core-shell structured metal powder with an oxide shell.

[0025] The beneficial effects of the present invention are:

[0026] (1) The present invention combines the two processes of preparing 1-10 μm spherical metal powder and insulating coating into one. First, the metal raw material is made into nano-scale metal powder, and then the nano-scale metal powder is heated to a molten state to increase the chance of collision, forming melt clusters to reach the desired size, and falling under the action of gravity. During the falling process, micron-scale molten spheres are formed under the action of surface tension, and then cooled to obtain micron-scale spherical metal powder. Subsequently, through surface energy and size effects, a layer of low melting point metal is adsorbed on the metal powder. During the passivation process, it reacts with oxygen to form an oxide insulating layer, thereby obtaining a 1-10 μm spherical core-shell structure metal powder.

[0027] (2) The present invention simultaneously adopts plasma arc-nanopowder growth-plasma arc composite technology to obtain micron-sized spherical powder with an insulating shell. At the same time, the present invention can adjust the collision probability to adjust the metal powder particle size, thereby solving the problems of metal powder core oxidation, low powder sphericity, and uncontrollable size. The obtained powder has a core-shell structure, the shell is a nano-scale thick oxide, the powder particle size is 1-10μm, the particle size distribution is narrow, and the sphericity is ≥95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 1 is a schematic structural diagram of a device for preparing 1-10 μm spherical core-shell structured metal powder according to Example 1 of the present invention;

[0029] Figure 2 is a schematic structural diagram of a nano powder generating device according to Embodiment 1 of the present invention;

[0030] Figure 3 Schematic diagram of the structure of the micron particle growth device of Example 1 of the present invention;

[0031] Figure 4 is a schematic structural diagram of a core-shell structure generating device according to Example 1 of the present invention;

[0032] Figure 5 is a schematic structural diagram of a passivation insulating collection device according to Embodiment 1 of the present invention;

[0033] Figure 6 is a schematic diagram of the growth process of 1-10 μm spherical core-shell structure metal powder according to Example 1 of the present invention;

[0034] Figure 7 It is a schematic diagram of the preparation of Fe@ZnO powder in Example 1 of the present invention;

[0035] Figure 8 is the HAADF diagram of the Fe@ZnO powder prepared in Example 1 of the present invention;

[0036] Fig. 9 This is the HAADF diagram of the FeNi@Al2O3 powder prepared in Example 2 of the present invention;

[0037] Fig.10 This is the HAADF diagram of the FeSi@SnO2 powder prepared in Example 3 of the present invention.

[0038] In the figure:

[0039] 1-nanopowder generating device, 11-arc chamber, 12-first feeding device, 121-feeding pipe, 122-feeding port, 123-discharging area, 13-first vacuum system, 14-gas path, 15-cooling system, 16-jet system, 161-jet pipe, 17-first electrode;

[0040] 2-micron particle growth device, 21-forming tube, 211-feed port, 212-discharge port, 213-air inlet, 22-first heating system, 23-first heat preservation system, 24-pneumatic system, air delivery pipe 241, 25-slow cooling pipe, 26-second heating system;

[0041] 3-core-shell structure generating device, 31-core-shell forming chamber, 32-second feeding device, 321-feeding pipe, 322-discharging port, 33-second heat preservation system, 34-second electrode, 35-transport pipeline, 36-powder feeding channel;

[0042] 4-passivation insulation collection device, 41-collection chamber, 42-second vacuum system, 43-passivation gas path, 44-powder inlet channel valve, 45-gas path valve;

[0043] 5-gas circulation device, 51-filter chamber, 52-circulating gas circuit, 53-blower. DETAILED DESCRIPTION

[0044] The following further describes the structures involved in the present invention or the technical terms used in these descriptions. These descriptions are only used as examples to illustrate how the methods of the present invention are implemented, and cannot constitute any limitation to the present invention.

[0045] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "back", "left" and "right" indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the positions or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limitations of the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0046] In the description of the present invention, unless otherwise clearly specified and limited, "connection", "fixation" and the like should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0047] The invention introduces a 1-10 μm spherical core-shell structure metal powder preparation device, comprising a nano powder generating device 1, a micron particle growth device 2, a core-shell structure generating device 3, a passivation insulation collecting device 4 and a gas circuit circulating device 5.

[0048] Nano powder generation device

[0049] like Figure 2 As shown, the plasma arc device 1 includes an arc chamber 11, a first feeding device 12, a first vacuum system 13, a gas circuit 14, a cooling system 15 and an injection system 16. A first electrode 17 is provided in the arc chamber 11, and the first vacuum system 13, the gas circuit 14, the cooling system 15 and the injection system 16 are respectively connected to the arc chamber 11.

[0050] As an optional embodiment, the material of the first electrode 17 is tungsten, graphite or niobium.

[0051] As an optional embodiment, the first feeding device 12 includes at least one feeding pipe 121, the feeding pipe 121 is horizontally arranged, and the feeding port 122 of the feeding pipe 121 is located 3 to 5 mm directly below the first electrode 17. Of course, the feeding pipe 121 is not limited to one, and can be two, three, or more. When there are multiple feeding pipes, the feeding pipes 121 are horizontally arranged and evenly arranged in concentric circles, and the circular area formed by the center of the circle is the discharge area 123, the first electrode 17 is located directly above the discharge area 123, and the diameter of the discharge area 123 is 3 to 5 mm.

[0052] As an optional embodiment, the gas introduced into the arc chamber 11 through the gas path 14 is one or more of nitrogen, argon, hydrogen, ammonia, etc.

[0053] As an optional embodiment, the gas injection system 16 injects gas at a certain pressure into the arc chamber 11, and the gas injection system 16 includes at least one gas injection pipe 161, and the angle formed with the horizontal line is 45° to 90°. Of course, the gas injection pipes 161 can be two, three, or more, and are evenly arranged in concentric circles with the first electrode 17 as the center.

[0054] As an optional embodiment, the gas injected into the arc chamber 11 by the injection system 16 is one or more of nitrogen, argon, hydrogen, and ammonia.

[0055] Functions of the nano-powder generating device: the arc chamber 11 is vacuumed through the first vacuum system 13, gas is introduced into the arc chamber 11 through the gas path 14 as a plasma atmosphere, and then a voltage is applied to the first electrode 17 to perform arc discharge on the high-melting-point metal raw material to make the metal raw material into nano-scale powder. At the same time, a gas with a certain pressure is sprayed into the arc chamber 11 by the jet system 16 to blow the nano-scale metal powder into the forming tube 21. The entire arc chamber 11 is cooled by the cooling system 15 to take away the heat.

[0056] Micron particle growth device

[0057] like Figure 3As shown, the micron particle growth device 2 includes a forming tube 21 , a first heating system 22 , a first heat preservation system 23 , a pneumatic system 24 , a slow cooling tube 25 and a second heating system 26 .

[0058] As an optional embodiment, the forming tube 21 is arranged vertically to reduce the metal powder from hitting the wall and adhering. The forming tube 21 has a feed port 211 and a discharge port 212, the feed port 211 is at the top and the discharge port 212 is at the bottom, the feed port 211 is connected to the arc chamber 11, the gas injected into the arc chamber 11 by the injection system 16 is directed toward the feed port 211, the first heating system 22 surrounds the forming tube 21 to heat the forming tube 21, at least the tube section between the feed port 211 and the discharge port 212 is surrounded by the first heating system 22, the forming tube 21 has an air inlet 213, the air inlet 213 is located between the feed port 211 and the discharge port 212, the pneumatic system 24 is connected to the air inlet 213 to inject a certain pressure of gas into the forming tube 21, and the gas direction is upward.

[0059] As an optional embodiment, the forming tube 21 is located directly below the feeding port 122, and the first electrode 17, the feeding port 122, and the forming tube 21 are on the same axis. In this way, it is convenient to directly and quickly feed the prepared nano-scale metal powder into the forming tube 21, so that sufficient nano-scale metal powder can be quickly and multiple times collided into a micron-scale melt in a molten state.

[0060] As an optional embodiment, the diameter of the forming tube 21 is not less than 60 mm and the length is not less than 1 meter.

[0061] As an optional embodiment, the forming tube 21 has a built-in clean lining made of high temperature resistant materials such as quartz, graphite, and stainless steel.

[0062] The density of the nano-scale solid metal powder in the forming tube is regulated by the air pressure injected by the jet system 16 and the diameter and length of the forming tube 21 to ensure the collision probability. The air pressure and the diameter and length of the forming tube 21 are set according to specific requirements.

[0063] As an optional embodiment, the pneumatic system 24 includes at least one air delivery pipe 241, the angle between the air delivery pipe 241 and the axis of the forming tube 21 downward is 0° to 45°, and the air inlet 213 is located at a position 1 / 2 to 2 / 3 downward of the forming tube 21. The air delivery pipes 241 can be two, three, or more, and are evenly arranged in concentric circles with the axis of the forming tube 21 as the center. The pneumatic force on the metal powder is determined by the angle between the air delivery pipe 241 and the forming tube 21 and the injection air pressure.

[0064] The air pressure injected by the pneumatic system 24 is used to adjust the residence time of the metal powder in the forming tube 21, thereby increasing the collision chance of the metal powder in the forming tube 21. The air pressure is set according to specific requirements.

[0065] As an optional embodiment, the discharge port 212 of the forming tube 21 is connected to the slow cooling tube 25, and the second heating system 26 heats the slow cooling tube 25 around the slow cooling tube 25. The heating temperature is higher than the melting point of the outer shell metal and lower than the melting point of the inner core metal, so that the inner core metal (high melting point micron-sized metal sphere) will not melt, and the outer shell metal (low melting point metal) is easy to adhere to the micron-sized sphere when in a molten state.

[0066] Function of the micron particle growth device 2: Nano-scale metal powder enters the forming tube 21, is heated into a molten state by the first heating system 22, and the pneumatic system 24 sprays the metal powder in the forming tube 21 to provide an upward support force for the metal powder, delay the descent of the metal powder, increase the collision of the metal powder, and then gather into micron-scale melt clusters and fall into the slow cooling tube 25 under the action of gravity, and form micron-scale spheres in the slow cooling tube 25 through surface tension, and the surface temperature of the micron-scale spheres is made higher than the melting point of the outer shell metal and lower than the melting point of the inner core metal under the heating of the second heating system 26.

[0067] Core-shell structure generation device

[0068] The core-shell structure generating device 3 comprises a core-shell molding chamber 31 , a second feeding device 32 connected to the core-shell molding chamber 31 , and a second heat preservation system 33 . A second electrode 34 is arranged in the core-shell molding chamber 31 . The core-shell molding chamber 31 is connected to the slow cooling pipe 25 .

[0069] Because the devices are interconnected to form an integrated device, the first vacuum system 13 and the gas path system 14 can be used to evacuate and inflate the entire device.

[0070] As an optional embodiment, the second feeding device 32 is arranged in the same structure as the first feeding device 12. The second feeding device 32 includes at least one feeding tube 321, the feeding tube 321 is arranged horizontally, and the outlet 322 of the feeding tube 321 is located 3 to 5 mm directly below the second electrode 34 to ensure rapid melting and sublimation of the low-melting-point metal. When multiple feeding tubes 321 are provided, the feeding tubes 321 are evenly arranged in concentric circles, and the circular area formed by the center of the circle is the feeding area. The second electrode 34 is located directly above the feeding area, and the diameter of the feeding area is 3 to 5 mm. The feed amount can be adjusted by the second feeding device 32 to control the volatilization amount of the low-melting-point metal, thereby controlling the thickness of the shell.

[0071] As an optional embodiment, a conveying pipe 35 connected to the slow cooling pipe 25 is provided in the core-shell molding chamber 31. The conveying pipe 35 changes diameter and gradually shrinks from top to bottom, allowing the micron-sized spheres to fall quickly. The second electrode 34 is arranged close to the conveying pipe 35, allowing the micron-sized spheres to appear concentrated near the second electrode 34.

[0072] Functions of the core-shell structure generating device 3: First, the low-melting-point metal raw material is rapidly melted and sublimated by the second feeding device 32 under the action of the second electrode 34, forming a low-melting-point metal atmosphere in the core-shell forming chamber 31. Secondly, the micron-sized spheres in the slow cooling tube 25 fall into the core-shell forming chamber 31 under the action of gravity, and the low-melting-point metal is adsorbed on the surface of the micron-sized spheres by means of surface energy and surface adsorption. Since the surface temperature of the micron-sized spheres is higher than the melting point of the low-melting-point metal, the metal adsorbed on the surface melts to form core-shell structure micron particles.

[0073] Passivation insulation collection device

[0074] The passivation insulating collection device 4 comprises a collection chamber 41 , a second vacuum system 42 connected to the collection chamber 41 , and a passivation gas path 43 . The collection chamber 41 is in communication with the core-shell molding chamber 31 .

[0075] As an optional embodiment, a passivation atmosphere is input into the collection chamber 41 through the passivation gas path 43. The passivation atmosphere may be an oxygen-containing atmosphere such as oxygen and air.

[0076] As an optional embodiment, the core-shell molding chamber 31 is connected to the collecting chamber 41 through the powder delivery channel 36, and a powder inlet channel valve 44 is provided on the powder delivery channel 36. The collecting chamber 41 can be arranged below or at the side of the core-shell molding chamber 31, and the core-shell structure micron particles are sucked into the collecting chamber 41 by the blower 53.

[0077] Function of the passivation insulation collection device 4: After the core-shell structure micron particles enter the collection chamber 41 through the powder delivery channel 36, the powder inlet channel valve 44 is closed, the second vacuum system 42 is opened, the collection chamber 41 is evacuated, and then the passivation atmosphere is input through the passivation gas path 43. Since the shell metal is at the nanometer scale and has a high surface activity, it is easy to react with the oxygen in the passivation atmosphere to form oxides, which play an insulating role on the micron particles. After cooling, they are collected.

[0078] Gas circulation device

[0079] The gas circulation device 5 includes a filter chamber 51 , a circulating gas path 52 and a blower 53 . The filter chamber 51 is connected to the collecting chamber 41 . The filter chamber 51 is connected to the arc chamber 11 through the circulating gas path 52 . The blower 53 is arranged on the circulating gas path 52 .

[0080] As an optional embodiment, a circulating gas circuit valve 45 is provided on the pipeline connecting the filter chamber 51 and the collection chamber 41 .

[0081] The nano powder generating device 1, the micron particle growing device 2, the core-shell structure generating device 3, and the passivation insulation collecting device 4 are carried out in the same closed cavity to ensure an oxygen-free environment.

[0082] The powder in the closed cavity is filtered out by the filter system 51, and a circulating gas path 52 is formed by the blower 53. Because the powder size is relatively small, there may be missed powder from the growth area to the collection area. If the powder is too small, it will affect the motor of the blower 53, so filtering is required to ensure the safety of the motor.

[0083] The high melting point metal includes but is not limited to pure metal, alloy, metal compound, etc., and the low melting point metal is pure metal.

[0084] Among them, the above-mentioned devices can be disassembled and used separately, or can be used in combination with existing equipment. For example, the method of making metal raw materials into nano-scale metal powder can be replaced by plasma arc discharge method, high-energy ball milling method, physical vapor deposition method, γ-ray radiation method, electrolysis method, etc., and melting can be replaced by laser melting, electron beam melting, etc.

[0085] The working process of the present invention is as follows: the high melting point metal raw material is fed into the first feeding device 12, which is sealed, the arc chamber 11 is evacuated through the first vacuum system 13, gas is introduced into the arc chamber 11 through the gas path 14 as a plasma atmosphere, a voltage is applied to the first electrode 17 to perform arc discharge on the metal raw material, and nano-scale metal powder is generated, and the nano-scale metal powder is blown into the forming tube 21 by the jet system 16. The nano-scale metal powder is heated to a molten state in the forming tube 21, and gas is sprayed into the gas system 24 to delay the descent of the powder, increase the collision chance of the powder in the forming tube 21, and aggregate into melt clusters until it grows to the required size and its gravity is greater than the gas force, and then it falls under the action of gravity, and forms micron-scale spheres through surface tension in the slow cooling tube 25, and the surface temperature of the micron-scale spheres is lower than the melting point of the inner metal and higher than the melting point of the outer shell metal under the heating of the second heating system 26. The micron-sized sphere enters the core-shell structure generating device 3 under the action of gravity, and the low-melting-point metal raw material is melted and sublimated through the second electrode 34 to form a low-melting-point metal atmosphere. With the help of surface adsorption, the low-melting-point metal gas is adsorbed on the surface of the micron-sized sphere and melted to form core-shell structure micron particles. It enters the passivation insulation collection device 4 through the powder delivery channel 36, and after the collection chamber 41 is closed, it is evacuated and flushed into the passivation atmosphere. Due to the nano-size effect of the shell metal, it reacts with the oxygen in the passivation atmosphere to generate oxides, which insulate the core-shell structure micron particles. After cooling, it is collected in the collection chamber 41. The powder in the closed cavity is filtered out by the filtering system 51, and a circulating gas path 52 is formed by the action of the blower 53.

[0086] The present invention also provides a method for preparing 1-10 μm spherical core-shell structure metal powder, which is prepared by the above-mentioned preparation device and comprises the following steps:

[0087] Step 1: The nano-powder generating device 1 converts the high melting point metal raw material into nano-scale metal powder, and blows the nano-scale metal powder into the forming tube 21 through the air injection system 16;

[0088] Step 2: The first heating system 22 heats the nano-scale metal powder into a molten state, and the pneumatic system 24 sprays gas at a certain pressure into the molding tube 21 to provide an upward supporting force. The molten metal powder collides and grows into a melt cluster until it reaches a desired size and the gravity is greater than the supporting force and falls into the slow cooling tube 25. During the falling process, micron-scale spherical metal powder is formed under the action of surface tension. The micron-scale spherical metal powder is then heated by the second heating system 26 to a surface temperature less than the melting point of the inner core metal and greater than the melting point of the outer shell metal, and enters the core-shell molding chamber 31;

[0089] Step 3: The low melting point metal raw material is made into a metal gas, whose melting point is lower than that of the high melting point metal. Under the surface adsorption force of the micron-sized spherical metal powder, the metal gas is adsorbed on the surface of the micron-sized spherical metal powder and melts to form micron-sized particles with a core-shell structure.

[0090] Step 4: The core-shell structured micron particles enter the collection chamber 41, and the passivation gas path 43 introduces a gas containing oxygen, and finally forms a 1-10 μm spherical core-shell structured metal powder with an oxide shell.

[0091] As an optional embodiment, in step 1, the method of preparing nano-scale metal powder from high melting point metal raw materials includes but is not limited to plasma arc discharge method, high energy ball milling method, physical vapor deposition method, γ-ray radiation method, electrolysis method, etc. Preferably, the plasma arc discharge method is used, and the voltage applied to the electrode is 20 to 600V.

[0092] The nano-scale metal powder is blown into the forming tube 21 through the air injection system 16. Since the nano-scale metal powder is light and in a floating state, a certain downward force needs to be provided to make the metal powder fall.

[0093] As an optional embodiment, in step 1, the closed environment for preparing the nano-scale metal powder is first evacuated and then gas is introduced, and the vacuum degree reaches at least 1×10 -3 Pa, the gas introduced is a mixture of Ar and H2, the Ar pressure is 0.009~0.09MPa, and the H2 pressure is 0.0009~0.009MPa.

[0094] As an optional embodiment, in step 2, the method of heating the nano-scale metal powder into a molten state includes but is not limited to arc heating, infrared heating, microwave heating, current magnetic effect heating, quartz tube heating, resistance heating, etc. Resistance heating is preferred, and the heating temperature is 1000°C to 1600°C.

[0095] As an optional embodiment, in step 2, measures to increase the probability of collision include setting up physical barriers, extending the length of the heating zone, using wind force, magnetic force, mechanical force, etc. in the opposite direction of gravity.

[0096] As an optional embodiment, in step 2, the supporting force is provided by, but not limited to, air force, magnetic force, mechanical force, etc. Air force is preferred, and the air pressure is 1-100 kPa Ar, indicating that the introduced gas is Ar.

[0097] As an optional embodiment, in step 4, the melting point of the low melting point metal is lower than the melting point of the high melting point metal, i.e., the micron-sized spherical metal powder by more than 400 degrees. The low melting point metal is preferably Al, Zn, Sn, etc.

[0098] As an optional embodiment, in step 4, the method for obtaining the low melting point metal includes but is not limited to plasma arc discharge method, induction heating method, laser heating method, etc. Preferably, the plasma arc discharge method is used, and the voltage applied to the electrode is 20-600V.

[0099] As an optional embodiment, in step 4, the passivation atmosphere is oxygen or an atmosphere containing oxygen, preferably air or oxygen.

[0100] As an optional embodiment, in step 5, the spherical core-shell structured metal powder obtained has an oxide shell with a shell thickness of nanometer level, a powder particle size of 1-10 μm, and a sphericity of ≥95%.

[0101] Example 1

[0102] like Figure 1-4 As shown, this embodiment introduces a 1-10μm spherical core-shell structure metal powder preparation device, including a nano powder generating device 1, a micron particle growth device 2, a core-shell structure generating device 3, a passivation insulation collecting device 4 and a gas circulation device 5.

[0103] The nano powder generating device 1 comprises an arc chamber 11, a first feeding device 12, a first vacuum system 13, a gas circuit 14, a cooling system 15 and an air injection system 16. A first electrode 17 is arranged in the arc chamber 11. The material of the first electrode 17 is tungsten. The first vacuum system 13, the gas circuit 14, the first cooling system 15 and the air injection system 16 are connected to the arc chamber 11 respectively.

[0104] The first feeding device 12 includes two feeding pipes 121, which are arranged horizontally and evenly in concentric circles, and the feeding port 122 of the feeding pipe 121 is located 4 mm directly below the first electrode 17. The circular area formed by the center of the circle is the discharge area 123, and the diameter of the discharge area 123 is 3 mm.

[0105] Two gas injection pipes 161 of the gas injection system 16 are provided, which are symmetrically arranged in concentric circles with the first electrode 17 as the center, and the angle between them and the horizontal line is 45°.

[0106] The micron particle growth device 2 comprises a forming tube 21 , a first heating system 22 , a first heat preservation system 23 , a pneumatic system 24 , a slow cooling tube 25 and a second heating system 26 .

[0107] The forming tube 21 is arranged vertically to reduce the metal powder from hitting the wall and adhering. The forming tube 21 has a feed port 211 and a discharge port 212, the feed port 211 is at the top, the discharge port 212 is at the bottom, the feed port 211 is connected to the arc chamber 11, the gas injected into the arc chamber 11 by the injection system 16 is directed toward the feed port 211, the first heating system 23 surrounds the forming tube 21 to heat the forming tube 21, the pipe section between the feed port 211 and the discharge port 212 is surrounded by the first heating system 23, the forming tube 21 has an air inlet 213, the air inlet 213 is located between the feed port 211 and the discharge port 212, the pneumatic system 24 is connected to the air inlet 213 to inject a certain pressure of gas into the forming tube 21, and the gas direction is upward. The air inlet 213 is at the 2 / 3 position of the forming tube 21 downward.

[0108] The forming tube 21 is located directly below the feeding port 122, and the first electrode 17, the feeding port 122, and the forming tube 21 are on the same axis. The forming tube 21 has a diameter of 80 mm and a length of 1.2 m. The forming tube 21 has a built-in clean lining made of quartz.

[0109] The pneumatic system 24 includes two air pipes 241, which are evenly arranged in concentric circles with the axis of the forming tube 21 as the center, and the angle between the air pipe 241 and the axis of the forming tube 21 is 42°. The discharge port 212 is connected to the slow cooling tube 25, and the second heating system 26 heats the slow cooling tube 25 around the slow cooling tube 25. The heating temperature is higher than the melting point of the shell metal and lower than the melting point of the core metal, so that the core metal (micron-sized spheres) will not melt, and the shell metal (low melting point metal) is easy to adhere to the micron-sized spheres when molten.

[0110] The core-shell structure generating device 3 comprises a core-shell molding chamber 31 , a second feeding device 32 connected to the core-shell molding chamber 31 , and a second heat preservation system 33 . A second electrode 34 is arranged in the core-shell molding chamber 31 . The core-shell molding chamber 31 is connected to the slow cooling pipe 25 .

[0111] The second feeding device 32 includes two feeding pipes 321, which are arranged horizontally and evenly in concentric circles, and the discharge ports 322 of the feeding pipes 321 are located 3 mm below the second electrode 34. The second electrode 34 is located above the feeding area 323, and the diameter of the feeding area 323 is 3 mm.

[0112] A delivery pipe 35 communicating with the slow cooling pipe 25 is disposed in the core-shell molding chamber 31 . The delivery pipe 35 changes diameter and gradually shrinks from top to bottom. The second electrode 34 is disposed close to the delivery pipe 35 .

[0113] The passivation insulation collection device 4 includes a collection chamber 41, a second vacuum system 42 connected to the collection chamber 41, and a passivation gas path 43. The collection chamber 41 is connected to the core-shell molding chamber 31. The passivation atmosphere is input into the collection chamber 41 through the passivation gas path 43. The core-shell molding chamber 31 is connected to the collection chamber 41 through the powder delivery channel 36, and the powder delivery channel valve 44 is provided on the powder delivery channel 36.

[0114] The collecting chamber 41 is located at the side of the core-shell molding chamber 31 . When the powder inlet channel valve 44 and the gas path valve 45 are opened, the blower 53 can form a circulating airflow to blow the powder into the collecting chamber 41 .

[0115] The nano powder generating device 1, the micron particle growing device 2, the core-shell structure generating device 3, and the passivation insulation collecting device 4 are carried out in the same closed cavity.

[0116] The gas circulation device 5 includes a filter chamber 51, a circulating gas circuit 52 and a blower 53. The filter chamber 51 is connected to the collection chamber 41. The filter chamber 51 is connected to the arc chamber 11 through the circulating gas circuit 52. The blower 53 is arranged on the circulating gas circuit 52. A circulating gas circuit valve 45 is arranged on the pipeline connecting the filter chamber 51 and the collection chamber 41.

[0117] This embodiment introduces a method for preparing 1-10 μm spherical core-shell structure metal powder using the above device, comprising the following steps:

[0118] Step 1: Put the rod-shaped Fe raw material into the first feeding device 12 of the nano-powder generating device 1, and evacuate the entire device through the first vacuum system 13, and the vacuum degree of the entire device reaches at least 1×10 -3 Pa, then Ar+H2 gas is introduced into the arc chamber 11 through the gas path 14, wherein the Ar gas pressure is 0.06MPa, the H2 gas pressure is 0.006MPa, and nano-Fe powder is prepared by plasma arc discharge, the voltage applied to the first electrode 17 is 50V, and the nano-Fe powder is blown into the molding tube 21 by spraying Ar gas using the injection system 16, and the gas pressure is 22kPa.

[0119] Step 2: The nanometer-scale Fe powder is heated to a molten state by the first heating system 22, and the heating temperature is 1300°C. Ar gas is sprayed into the forming tube 21 by the pneumatic system 24 to delay the descent of the metal powder. The gas pressure is 20 kPa. The Fe powder collides and grows into melt clusters until the gravity reaches the required size is greater than the supporting force and falls into the slow cooling tube 25. During the falling process, micron-scale spherical Fe powder is formed by surface tension. Then, the surface temperature of the micron-scale spherical Fe powder is made greater than the melting point of the outer shell metal and less than the melting point of the inner core metal by the second heating system 26. The heating temperature is 800°C and the powder enters the core-shell forming chamber 31.

[0120] Step 3: The rod-shaped Zn raw material is fed into the core-shell molding chamber 31 through the second feeding device 32, and a metal Zn atmosphere is produced by plasma arc discharge. The voltage applied to the second electrode 34 is 120V. The melting point of the micron-sized spherical Fe powder is higher than the melting point of Zn. Under the surface adsorption force of the Fe powder, the Zn gas is adsorbed on the surface of the micron-sized spherical Fe powder and melts to form micron-sized particles with a core-shell structure.

[0121] Step 4: The core-shell structured micron particles enter the collection chamber 41 and are evacuated by the second vacuum system 42 to a vacuum degree of at least 1 Pa. Oxygen is then introduced through the passivation gas path 43 for passivation. After being cooled to room temperature, the particles can be screened and packaged.

[0122] The obtained Fe@ZnO powder (denoting ZnO coated Fe) has a complete core-shell structure, with the outer shell being ZnO, a thickness of ~14 nm, a powder particle size of 3.5 μm, and a sphericity of ≥95%, see Figure 7 , 8 .

[0123] Example 2

[0124] The difference between this embodiment and embodiment 1 is that:

[0125] The jet pipe 161 of the jet system 16 is at an angle of 60° to the horizontal line. The diameter of the forming tube 21 is 60 mm and the length is 1 meter. The forming tube 21 is installed with a clean liner made of graphite. The angle between the air delivery pipe 241 and the axis of the forming tube 21 downward is 30°. The air inlet 213 is at the 1 / 2 position downward of the forming tube 21. The rest is the same as in Example 1.

[0126] The preparation method of 1-10μm spherical core-shell structure metal powder is as follows:

[0127] Step 1: Place the rod-shaped FeNi raw material into the first feeding device 12 of the nanopowder generating device 1, seal the entire device, and evacuate the entire device through the first vacuum system 13. The vacuum degree of the entire device reaches at least 1×10 -3Pa, Ar+H2 gas is introduced into the arc chamber 11 through the gas path 14, wherein the Ar gas pressure is 0.09MPa, and the H2 gas pressure is 0.007MPa, a voltage of 250V is applied to the first electrode 17 to perform arc discharge on the high melting point metal raw material to prepare nano-FeNi powder, and Ar gas is sprayed by the injection system 16 to blow the nano-FeNi powder into the molding tube 21, and the gas pressure is 30KPa.

[0128] Step 2: The nanometer-scale FeNi powder is heated to a molten state by the first heating system 22, and the heating temperature is 1100°C. Ar gas is sprayed into the forming tube 21 by the pneumatic system 24 to delay the descent of the powder. The gas pressure is 30KPa. The FeNi powder collides and grows into melt clusters until the gravity reaches the required size is greater than the supporting force and falls into the slow cooling tube 25, and micron-scale spherical FeNi powder is formed by surface tension. The surface temperature of the micron-scale spherical FeNi powder is greater than the melting point of the outer shell metal and less than the melting point of the inner core metal by the second heating system 26. The heating temperature is 800°C and enters the core-shell molding chamber 31.

[0129] Step 3: The rod-shaped Al raw material is fed into the core-shell molding chamber 31 through the second feeding device 32, and a voltage of 250V is applied to the second electrode 34 to perform arc discharge on the rod-shaped Al, thereby forming an Al atmosphere in the core-shell molding chamber 31. The surface temperature of the micron-sized spherical FeNi powder is higher than the melting point of Al. Under the surface adsorption force of the FeNi powder, the Al gas is adsorbed on the surface of the micron-sized spherical FeNi powder and melts to form micron-sized particles with a core-shell structure.

[0130] Step 4: After the core-shell structured micron particles enter the collection chamber 41, they are evacuated to 5 Pa by the second vacuum system 42, and then air is input through the passivation gas path 43 for passivation. After being cooled to room temperature, they can be screened and packaged.

[0131] The obtained FeNi@Al2O3 powder has a complete core-shell structure, with an outer shell of Al2O3, a thickness of ~16nm, a powder particle size of 1.4μm, and a sphericity of ≥95%, see Fig. 9 .

[0132] Example 3

[0133] The difference between this embodiment and embodiment 1 is that:

[0134] The angle between the jet pipe 161 of the jet system 16 and the horizontal line is 80°. The diameter of the discharge area 123 is 5 mm. The diameter of the forming tube 21 is 70 mm and the length is 1.0 m. The angle between the air delivery pipe 241 and the axis of the forming tube 21 downward is 40°. Others are the same as in Example 1.

[0135] The preparation method of 1-10μm spherical core-shell structure metal powder is as follows:

[0136] Step 1: Place the rod-shaped FeSi raw material into the first feeding device 12 of the nanopowder generating device 1, seal the entire device, and evacuate the entire device through the first vacuum system 13. The vacuum degree of the entire device reaches at least 1×10 -3 Pa, then Ar+H2 gas is introduced into the arc chamber 11 through the gas path 14, wherein the Ar gas pressure is 0.07MPa, the H2 gas pressure is 0.007MPa, and nano-scale solid FeSi powder is prepared by plasma arc discharge, the voltage applied to the first electrode 17 is 20V, and the nano-scale FeNi powder is blown into the molding tube 21 by spraying Ar gas using the injection system 16, and the gas pressure is 25KPa.

[0137] Step 2: The nanometer-scale FeSi powder is heated to a molten state at a temperature of 1200°C by the first heating system 22, and Ar gas is sprayed into the molding tube 21 through the pneumatic system 24 to delay the descent of the powder. The gas pressure is 25 kPa, and the FeSi powder collides and grows into melt clusters until the gravity reaches the required size is greater than the supporting force and falls into the slow cooling tube 25, and micron-scale spherical FeSi powder is formed by surface tension. The surface temperature of the micron-scale spherical FeSi powder is greater than the melting point of the outer shell metal and less than the melting point of the inner core metal by the second heating system 26. The heating temperature is 800°C and enters the core-shell molding chamber 31.

[0138] Step 3: The rod-shaped Sn raw material is fed into the core-shell molding chamber 31 through the second feeding device 32, and a metal Sn atmosphere is produced by plasma arc discharge. The voltage applied to the second electrode 34 is 200 V. Under the surface adsorption force of the FeSi powder, the Sn gas is adsorbed on the surface of the micron-sized spherical FeSi powder and melts to form micron-sized particles with a core-shell structure.

[0139] Step 4: After the core-shell structured micron particles enter the collection chamber 41, they are evacuated to 5 Pa by the second vacuum system 42, and then air is input through the passivation gas path 43 for passivation. After being cooled to room temperature, they can be screened and packaged.

[0140] The obtained FeSi@SnO2 powder has a complete core-shell structure, with the outer shell being SiO2, the thickness being ~18nm, the powder particle size being 1.8μm, and the sphericity being ≥95%, see Fig.10 .

[0141] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A device for preparing 1-10 μm spherical core-shell structure metal powder, characterized by: include: A nano powder generating device (1), comprising an arc chamber (11) and a first feeding device (12) connected to the arc chamber (11), a first vacuum system (13), a gas path (14), a cooling system (15) and an injection system (16); a first electrode (17) is provided inside the arc chamber (11); A micron particle growth device (2), the micron particle growth device (2) comprising a forming tube (21), a first heating system (22), a first heat preservation system (23), a pneumatic system (24), a slow cooling tube (25) and a second heating system (26); the forming tube (21) is arranged vertically, and has a feed port (211) and a discharge port (212); the feed port (211) is at the top, and the discharge port (212) is at the bottom; the feed port (211) is connected to an arc chamber (11); the first heating system (22) and the first heat preservation system (23) are arranged outside the forming tube (21); the pneumatic system (24) is connected to the forming tube (21) to spray a gas of a certain pressure into the forming tube (21) and the gas direction is upward; the discharge port (212) is connected to the slow cooling tube (25); the second heating system (26) is arranged outside the slow cooling tube (25); A core-shell structure generating device (3), the core-shell structure generating device (3) comprising a core-shell forming chamber (31) and a second feeding device (32) and a second heat preservation system (33) connected to the core-shell forming chamber (31), a second electrode (34) being arranged in the core-shell forming chamber (31), and the core-shell forming chamber (31) being connected to a slow cooling pipe (25); A passivation insulating collection device (4), the passivation insulating collection device (4) comprising a collection chamber (41) and a second vacuum system (42) and a passivation gas path (43) connected to the collection chamber (41), the collection chamber (41) being in communication with the core-shell molding chamber (31).

2. The 1-10 μm spherical core-shell structure metal powder preparation device according to claim 1, characterized in that: The first feeding device (12) comprises at least one feeding pipe (121), the feeding pipe (121) is arranged horizontally, and the feeding port (122) of the feeding pipe (121) is located 3 to 5 mm below the first electrode (17); when multiple feeding pipes (121) are provided, the feeding pipes (121) are evenly arranged in concentric circles, and the circular area formed with the center of the circle is the discharge area (123), the first electrode (17) is located directly above the discharge area (123), and the diameter of the discharge area (123) is 3 to 5 mm.

3. The 1-10 μm spherical core-shell structure metal powder preparation device according to claim 2, characterized in that: The diameter of the forming tube (21) is not less than 60 millimeters and the length is not less than 1 meter. The forming tube (21) is located directly below the feeding port (122), and the first electrode (17), the feeding port (122) and the forming tube (21) are located on the same axis.

4. The 1-10 μm spherical core-shell structure metal powder preparation device according to claim 3, characterized in that: The jet system (16) comprises at least one jet pipe (161), the angle formed with the horizontal line being 45° to 90°.

5. The 1-10 μm spherical core-shell structure metal powder preparation device according to claim 1, characterized in that: The forming tube (21) has an air inlet (213), and the air inlet (213) is located between the feed port (211) and the discharge port (212). The pneumatic system (23) is connected to the air inlet (213), and the air inlet (213) is located at a 1 / 2 to 2 / 3 position downward of the forming tube (21).

6. The device for preparing 1-10 μm spherical core-shell structure metal powder according to claim 5, characterized in that: The pneumatic system (24) comprises at least one air delivery pipe (241), wherein the angle formed downwardly by the air delivery pipe (241) and the axis of the forming pipe (21) is 0° to 45°.

7. The 1-10 μm spherical core-shell structure metal powder preparation device according to claim 1, characterized in that: The second feeding device (32) comprises at least one feeding pipe (321), the feeding pipe (321) is arranged horizontally, and the discharge port (322) of the feeding pipe (321) is located 3 to 5 mm below the second electrode (34).

8. The device for preparing 1-10 μm spherical core-shell structure metal powder according to claim 1, characterized in that: A delivery pipe (35) communicating with the slow cooling pipe (25) is provided in the core-shell molding chamber (31); the delivery pipe (35) changes diameter and gradually shrinks from top to bottom; and the second electrode (34) is arranged close to the delivery pipe (35).

9. The device for preparing 1-10 μm spherical core-shell structure metal powder according to claim 1, characterized in that: The nano powder generating device (1), the micron particle growth device (2), the core-shell structure generating device (3) and the passivation insulation collecting device (4) are in the same closed cavity; the metal powder preparing device comprises an air circulation device (5), the air circulation device (5) comprises a filter chamber (51), a circulating air path (52) and a blower (53), the filter chamber (51) is connected to the collecting chamber (41), the filter chamber (51) is connected to the arc chamber (11) via the circulating air path (52), and the blower (53) is arranged on the circulating air path (52).

10. A method for preparing 1-10 μm spherical core-shell structure metal powder, characterized in that: The metal powder preparation device according to any one of claims 1 to 9 is prepared, comprising the following steps: Step 1: The nano powder generating device (1) converts the high melting point metal raw material into nano metal powder, and blows the nano metal powder into the forming tube (21) through the air injection system (16); Step 2: The first heating system (22) heats the nano-scale metal powder into a molten state, and the pneumatic system (24) sprays gas at a certain pressure into the molding tube (21) to provide an upward supporting force. The molten metal powder collides and grows into a melt cluster until it reaches a desired size and the gravity is greater than the supporting force and falls into the slow cooling tube (25). During the falling process, micron-scale spherical metal powder is formed under the action of surface tension. The micron-scale spherical metal powder is then heated by the second heating system (26) to a surface temperature less than the melting point of the inner core metal and greater than the melting point of the outer shell metal, and enters the core-shell molding chamber (31); Step 3: The low melting point metal raw material is made into metal gas, whose melting point is lower than that of the high melting point metal. Under the surface adsorption force of the micron-sized spherical metal powder, the metal gas is adsorbed on the surface and melted to form micron particles with core-shell structure; Step 4: The core-shell structured micron particles enter the collection chamber (41), and a gas containing oxygen is introduced into the passivation gas path (43), and finally a 1-10 μm spherical core-shell structured metal powder with an oxide shell is formed.

Citation Information

Patent Citations

  • Insulating coated soft magnetic powder

    CN117396989A

  • Microfiller-inlaid flexible silicon dioxide nanofiber membrane and preparation method thereof

    CN118910813A

Cited By

  • Device and method for preparing submicron powder with core-shell structure by compounding heat preservation type plasma arc-spray coating

    CN119772189A

  • An apparatus and method for preparing submicron powder with core-shell structure by thermal-insulated plasma arc-spray coating composite

    CN119772189B