Titanium steel dissimilar metal and processing method thereof
By using unequal thickness Cu foil, V foil superimposed composite intermediate material and efficient ytterbium-doped fiber laser in titanium/steel differential metal laser welding, the formation of Ti-Fe and Cu-Ti brittle phases is prevented, and titanium is significantly improved /Mechanical properties of steel different metal welded joints.
Patent Information
- Application Number
- CN202411416373.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The prior art is difficult to effectively prevent the formation of Ti-Fe brittle intermetallic compounds in titanium/steel different metal laser welding, resulting in limited improvement in the mechanical properties of the joints.
Using unequal thickness Cu foil and V foil as composite intermediate layer material, the laser power and speed are adjusted through overlapping structure and efficient ytterbium-doped fiber laser welding to ensure that the vanadium foil is not completely melted, hindering the diffusion of the base material element and avoiding Ti -Fe and Cu-Ti brittle phase formation.
The mechanical properties of titanium/steel different metal welded joints are significantly improved, the formation of Ti-Fe and Cu-Ti brittle phases is avoided, and the tensile strength and ductility of the joints are enhanced.
Smart Images

Figure CN119057241A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of welding (connection) of dissimilar materials, and in particular relates to a titanium steel dissimilar metal and a processing method thereof, which are applied to technical fields such as new energy vehicles, aerospace, and nuclear power industry. Background Art
[0002] The heterogeneous composite structure prepared by welding titanium alloy and steel combines the good corrosion resistance and high specific strength of titanium alloy and the excellent comprehensive performance, easy processing and low cost of steel. As a typical heterogeneous structure, it has a wide application background and prospects in new energy vehicles, medical equipment, aerospace, nuclear power industry, etc. However, the welded joints prepared by titanium / steel dissimilar metals are prone to form Ti-Fe brittle intermetallic compounds, and due to the obvious differences in the physical and chemical properties of the two, the residual stress of the joint after welding is large, resulting in low mechanical properties of the joint.
[0003] In the process of implementing the present invention, the inventors found that the prior art has at least the following problems:
[0004] The existing technology adds a single intermediate layer material such as Cu, Ni, V, etc., which can reduce the content of Ti-Fe brittle intermetallic compounds in titanium / steel laser welded joints to a certain extent and improve the mechanical properties of the joints. However, the addition of a single intermediate layer material cannot prevent the mutual diffusion of Ti and Fe elements in the parent material during the welding process, and a certain amount of Ti-Fe brittle phase is still formed in the joints. Therefore, the mechanical properties of the joints prepared by titanium / steel dissimilar metal laser welding by adding a single intermediate layer material are limited.
[0005] CN104028914A-Welding wire for welding titanium-pipeline steel composite plate near steel layer and preparation method thereof, discloses a welding wire for welding titanium-pipeline steel composite plate near steel layer, which is composed of the following components by mass percentage: Si2.7-3.3%, Mn1.2-1.8%, C≤0.04%, P≤0.007%, S≤0.035%, the remainder is Cu, and the sum of the mass percentages of each component is 100%. It also cannot solve the above technical problems. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a titanium-steel dissimilar metal and a processing method thereof. Aiming at the problem of a large amount of Ti-Fe binary brittle phase in titanium / steel dissimilar joints, a laser beam is used as a welding heat source, Cu foil and V foil of different thickness are superimposed as a composite intermediate layer material, and the welding structure is in the form of overlap. By adjusting and optimizing the laser process parameters, a stainless steel-copper-vanadium (not fully melted)-titanium alloy welding joint is obtained. Since the V foil is not completely melted during the welding process, it will effectively hinder the diffusion of the parent material elements on both sides, avoid the formation of Ti-Fe binary brittle phase in the joint, and at the same time hinder the downward diffusion of Cu elements and the combination with Ti elements to produce Cu-Ti binary brittle phase, thereby greatly improving the mechanical properties of the joint.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a titanium steel dissimilar metal, the materials are overlapped and placed in the order of stainless steel, copper foil, vanadium foil, and titanium alloy from top to bottom, and the overlapping areas are welded to fuse the materials.
[0008] After the materials are placed, use clamps to clamp them to maintain compression between the materials.
[0009] The fixture has a bottom plate, and the stainless steel, copper foil, vanadium foil, and titanium alloy are placed on the bottom plate in sequence; clamping plates are provided on both sides of the bottom plate, and the clamping plates are connected to the bottom plate through fastening nuts, and the clamping plates can clamp the materials.
[0010] The vanadium foil is 0.05 mm thick, and the copper foil is 0.03 mm thick.
[0011] The titanium steel dissimilar metal processing method adopts a welding process, and the welding is performed by a high-efficiency ytterbium-doped fiber laser.
[0012] During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-vanadium foil weld and a vanadium foil-titanium alloy weld.
[0013] In order to prevent the Fe and Ti elements in the stainless steel and titanium alloy base materials from diffusing each other, the welding speed and laser power were adjusted to prevent the vanadium foil middle layer from completely melting. After welding, a joint consisting of a weld formed by the melting of stainless steel-copper, copper-vanadium, an incompletely melted vanadium foil and a weld formed by heat conduction of vanadium-titanium alloy was obtained.
[0014] The high-efficiency ytterbium-doped fiber laser has a laser power of 2800W-3000W and a defocus amount of 0.
[0015] The laser emission angle is 9°-12° to the material surface.
[0016] The laser welding speed is 30 mm / s. Through welding, a weld joint consisting of a stainless steel-copper weld formed by melting, and a copper-vanadium and vanadium-titanium alloy weld formed by heat conduction is formed.
[0017] One of the above technical solutions has the following advantages or beneficial effects: in view of the problem of a large amount of Ti-Fe binary brittle phase in titanium / steel dissimilar joints, a laser beam is used as a welding heat source, Cu foil and V foil of different thickness are superimposed as a composite intermediate layer material, and the welding structure is in the form of overlap. By adjusting and optimizing the laser process parameters, a stainless steel-copper-vanadium (not fully melted)-titanium alloy welded joint is obtained. Since the V foil is not completely melted during the welding process, it will effectively hinder the diffusion of the parent material elements on both sides, avoid the formation of Ti-Fe binary brittle phase in the joint, and at the same time hinder the downward diffusion of Cu elements and the combination with Ti elements to produce Cu-Ti binary brittle phase, thereby greatly improving the mechanical properties of the joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A schematic diagram of a welding structure and a welding process of titanium steel dissimilar metals and a processing method thereof provided in an embodiment of the present invention;
[0019] Figure 2 The microstructure morphology of the titanium alloy-stainless steel joint of the present invention is as follows: (a) a low-magnification photograph of a cross section of a stainless steel-copper-vanadium-titanium alloy weld, (b) a high-magnification photograph of a cross section of a stainless steel-copper-vanadium-titanium alloy weld near the stainless steel side at the center, (c) a high-magnification photograph of a cross section of a stainless steel-copper-vanadium-titanium alloy weld near the titanium alloy side at the center;
[0020] Figure 3 It is a schematic diagram of the preparation process of the titanium alloy-stainless steel welded joint of the present invention.
[0021] The marks in the above figures are: 1. positioning base plate, 2. pressing plate, 3. tightening adjustment nut, 4. stainless steel plate, 5. titanium alloy plate, 6. Cu, V foil composite middle layer. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Embodiment 1
[0024] See also Figures 1 to 3, a titanium steel dissimilar metal, the materials are overlapped and placed in the order of stainless steel 4, copper foil, vanadium foil, and titanium alloy 5 from top to bottom, and the overlapping areas are welded to fuse the materials. After the materials are placed, they are clamped with a clamp to maintain a certain clamping force between the contact surfaces of the welding base material and the intermediate layer material. The welding structure of stainless steel 4-copper-vanadium-titanium alloy 5 overlapped from top to bottom only needs one welding to obtain a welded joint under the action of heat conduction.
[0025] The fixture has a bottom plate 1, stainless steel 4, copper foil, vanadium foil, and titanium alloy 5 are placed on the bottom plate 1 in sequence; clamping plates 2 are provided on both sides of the bottom plate 1, and the clamping plates 2 are connected to the bottom plate 1 through fastening nuts 3, and the clamping plates 2 can clamp the materials. After the materials are placed, they are clamped with the fixture to maintain a certain clamping force between the contact surfaces of the welding base material and the intermediate layer material.
[0026] The thickness of the vanadium foil is 0.05mm, and the thickness of the copper foil is 0.03mm. The thickness of the copper and vanadium foils in the composite intermediate layer is controlled separately, which not only ensures that the vanadium foil is not completely melted, thereby hindering the mutual diffusion of Ti and Fe elements in the parent material, but also forms an effective welding joint.
[0027] The processing method adopts welding technology, and the welding adopts high-efficiency ytterbium-doped fiber laser for welding. By optimizing the process parameters and improving the joint performance, the goal is to obtain the best weld morphology and avoid defects such as pores, spatter, and cracks. The welded joint obtained by laser welding has good surface morphology, uniform weld, no defects such as pores, spatter, cracks, and incomplete penetration, and good welding process performance.
[0028] During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel 4-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-vanadium foil weld and a vanadium foil-titanium alloy 5 weld.
[0029] In order to prevent the Fe and Ti elements in the stainless steel 4 and the titanium alloy 5 from diffusing each other, the welding speed and laser power were adjusted to prevent the vanadium foil middle layer from completely melting. After welding, a joint consisting of a weld formed by the melting of stainless steel 4-copper, copper-vanadium, an incompletely melted vanadium foil and a weld formed by heat conduction of vanadium-titanium alloy 5 was obtained.
[0030] Since copper foil has good ductility and plasticity, the stress of the joint is relieved during welding and cooling, thereby improving the mechanical properties of the joint. The tensile strength of the composite welded joint composed of the weld formed by melting stainless steel 4-copper and the weld formed by heat conduction of copper-vanadium and vanadium-titanium alloy 5 reaches 380-410MPa.
[0031] The laser power of the high-efficiency ytterbium-doped fiber laser is 2800W-3000W, and the defocus is 0. The laser emission angle is 9°-12° with the material surface. The laser welding speed is 30mm / s. Through welding, a weld joint consisting of a weld formed by melting stainless steel 4-copper and a weld formed by heat conduction of copper-vanadium and vanadium-titanium alloy 5 is formed. By accurately adjusting the parameters such as laser power, intermediate layer thickness and welding speed, the Ti-Fe binary brittle phase is controlled not to be formed in the stainless steel 4-vanadium-copper-titanium alloy 5 weld joint. When the thickness of the composite intermediate layer is kept constant at 0.05 mm vanadium foil and 0.03 mm copper foil, the welding speed is 30 mm / s, and the defocus is 0, when the laser power is 2800 W, no Ti-Fe phase is found in the weld area. On the side near the stainless steel 4, the molten vanadium foil and the two base materials form a large amount of (Fe, V), (Cr, V) solid solution and a small amount of CuTi2 brittle phase. On the side near the titanium alloy 5, a (β-Ti, V) solid solution is formed, and the joint is more brittle. When the laser power is 3000 W, the welding power is high and the heat input is low. When the laser power is too large, cracks will appear in the joint and expand, which has no application value. When the laser power is 2900W, no Ti-Fe phase is found in the weld area. On the side near the stainless steel 4, the molten vanadium foil and the two parent materials form a large amount of (Fe, V) and (Cr, V) solid solutions. On the side near the titanium alloy 5, a large amount of (β-Ti, V) solid solutions and a small amount of Cu-Al tough phase are formed, and the brittleness of the joint is reduced. At the same time, because the copper foil has quite good ductility and plasticity, the stress of the joint is relieved during the welding and cooling process, thereby significantly improving the mechanical properties.
[0032] The incompletely melted vanadium intermediate layer will effectively prevent the diffusion and combination of Ti, Fe, Cu, and Ti elements, thereby avoiding the formation of Ti-Fe and Cu-Ti binary brittle phases in the joint. At the same time, the laser power and welding speed are strictly controlled to form a solid solution of (Fe, V), (Cr, V), and (β-Ti, V) in the joint. At the same time, since the copper foil has quite good ductility and plasticity, the stress of the joint is relieved during the welding and cooling process, thereby improving the mechanical properties of the joint.
[0033] Through the innovative titanium / steel dissimilar metal laser thermal welding with an overlapping structure and an unequally thick copper-vanadium composite intermediate layer, a better titanium / steel dissimilar metal overlapping laser welding joint is prepared. Through the titanium / steel dissimilar metal laser thermal welding process with an overlapping structure and an unequally thick copper-vanadium composite intermediate layer, the organization in the titanium / steel dissimilar metal welding joint is optimized, its weldability is improved, and the mechanical properties of the joint are improved. This titanium / steel dissimilar metal laser thermal welding process with an overlapping structure and an unequally thick copper-vanadium composite intermediate layer is original in the field of dissimilar material welding (connection).
[0034] Embodiment 2
[0035] The titanium / steel dissimilar metal laser welding process method of the present invention, which adds a composite intermediate layer of Cu and V foils of unequal thickness, aims at the problem of a large amount of Ti-Fe binary brittle phase in titanium / steel dissimilar joints. The laser beam is used as the welding heat source, and Cu foils and V foils of unequal thickness are superimposed as the composite intermediate layer material. The welding structure adopts the form of overlap. By adjusting and optimizing the laser process parameters, the formation of Ti-Fe binary brittle phase in the joint is effectively avoided, thereby greatly improving the mechanical properties of the joint. Laser thermal conduction welding is adopted to obtain a high-quality welded joint composed of a weld formed by melting stainless steel-copper, a weld formed by heat conduction of an incompletely melted vanadium foil, and copper-vanadium and copper-titanium alloys. The process steps are: stack and place each material according to the designed welding structure → lock the contact surfaces of each material with a locking adjustment nut → weld by irradiating the laser once on the stainless steel surface, thereby realizing the connection of titanium alloy and stainless steel dissimilar materials. The specific steps are as follows:
[0036] (1) Welding structure: The welding base material and the intermediate layer material are overlapped and placed in the order of stainless steel, copper foil, vanadium foil, and titanium alloy from top to bottom. After placement, they are clamped with a clamp to maintain a certain compression force between the contact surfaces of the welding base material and the intermediate layer material;
[0037] (2) Welding process: Welding is performed using a high-efficiency ytterbium-doped fiber laser. The laser emission angle is 9°-12° to the material surface. The laser power is 2800W-3000W. The welding speed is 30mm / s. The defocus is 0. The joint performance is improved through welding to obtain the optimal weld morphology and avoid defects such as pores, spatter, and cracking.
[0038] (3) When welding, the laser emission angle is adjusted to weld the overlapping area to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-vanadium foil weld and a vanadium foil-titanium alloy weld;
[0039] (4) The incomplete melting of the vanadium foil intermediate layer in the weld joint allows the diffusion and combination of Fe, Ti, Cu, and Ti elements in the stainless steel and titanium alloy base materials, thereby avoiding the formation of Ti-Fe and Cu-Ti binary brittle phases in the joint.
[0040] By precisely adjusting the laser power, the thickness of the intermediate layer, and the welding speed, the Ti-Fe binary brittle phase is prevented from forming in the stainless steel-vanadium-copper-titanium alloy welded joint. When the thickness of the composite intermediate layer is kept constant at 0.05mm vanadium foil and 0.03mm copper foil, the welding speed is 30mm / s, and the defocus is 0, when the laser power is 2800W, no Ti-Fe phase is found in the weld area. On the stainless steel side, the molten vanadium foil forms a large amount of (Fe, V), (Cr, V) solid solution and a small amount of CuTi2 brittle phase with the two base materials. On the titanium alloy side, a (β-Ti, V) solid solution is formed, and the joint is more brittle. When the laser power is 3000W, the welding power is high and the heat input is low. If the laser power is too large, cracks will appear in the joint and expand, which has no application value. When the laser power is 2900W, no Ti-Fe phase is found in the weld area. On the stainless steel side, the molten vanadium foil and the two parent materials form a large amount of (Fe, V) and (Cr, V) solid solutions. On the titanium alloy side, a large amount of (β-Ti, V) solid solutions and a small amount of Cu-Al tough phase are formed, and the brittleness of the joint is reduced. At the same time, since the copper foil has quite good ductility and plasticity, the stress of the joint is relieved during welding and cooling, thereby significantly improving the mechanical properties.
[0041] Laser thermal conduction welding is used, and the welding process parameters are precisely adjusted so that the laser irradiates the stainless steel surface. A high-quality welded joint consisting of a weld formed by melting stainless steel-copper, an incompletely melted vanadium foil, and a weld formed by heat conduction of copper-vanadium and copper-titanium alloys is prepared in one welding. Since the vanadium foil intermediate layer is not completely melted, the mutual diffusion and combination of Ti and Fe elements are effectively blocked, and the formation of Ti-Fe binary brittle phase is avoided. In addition, the heat input is controlled by controlling the laser power, and the amount of vanadium and copper elements is controlled by controlling the thickness of the vanadium foil and copper foil in the composite intermediate layer respectively, and the copper foil is placed on top in space, so as to avoid the appearance of Cu-Ti binary brittle phase as much as possible. At the same time, since the copper foil has quite good ductility and plasticity, the stress of the joint is relieved during the welding and cooling process, thereby significantly improving the mechanical properties.
[0042] After adopting the above scheme, in order to solve the problem of a large number of Ti-Fe binary brittle phases in titanium / steel dissimilar joints, a laser beam is used as a welding heat source, Cu foil and V foil of different thicknesses are superimposed as composite intermediate layer materials, and the welding structure is overlapped. By adjusting and optimizing the laser process parameters, a stainless steel-copper-vanadium (not fully melted)-titanium alloy welded joint is obtained. Since the V foil is not completely melted during the welding process, it will effectively hinder the diffusion of the parent material elements on both sides, avoid the formation of Ti-Fe binary brittle phases in the joint, and at the same time hinder the downward diffusion of Cu elements and the combination with Ti elements to produce Cu-Ti binary brittle phases, thereby greatly improving the mechanical properties of the joint.
[0043] In the description of the present invention, it is necessary to understand that the terms "coaxial", "bottom", "one end", "top", "middle", "the other end", "upper", "one side", "top", "inside", "front", "center", "both ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0044] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.
[0045] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A titanium steel dissimilar metal, characterized in that: The materials are overlapped and placed in the order of stainless steel, copper foil, vanadium foil and titanium alloy from top to bottom, and the overlapping areas are welded to fuse the materials.
2. The titanium steel dissimilar metal according to claim 1, characterized in that: After the materials are placed, use clamps to clamp them to maintain compression between the materials.
3. The titanium steel dissimilar metal according to claim 2, characterized in that: The fixture has a bottom plate, and the stainless steel, copper foil, vanadium foil, and titanium alloy are placed on the bottom plate in sequence; clamping plates are provided on both sides of the bottom plate, and the clamping plates are connected to the bottom plate through fastening nuts, and the clamping plates can clamp the materials.
4. The titanium steel dissimilar metal according to claim 3, characterized in that: The vanadium foil is 0.05 mm thick, and the copper foil is 0.03 mm thick.
5. The titanium steel dissimilar metal processing method according to any one of claims 1 to 4, characterized in that: The processing method adopts welding technology, and the welding adopts high-efficiency ytterbium-doped fiber laser for welding.
6. The titanium steel dissimilar metal according to claim 5, characterized in that: During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-vanadium foil weld and a vanadium foil-titanium alloy weld.
7. The titanium steel dissimilar metal according to claim 6, characterized in that: In order to prevent the Fe and Ti elements in the stainless steel and titanium alloy base materials from diffusing each other, the welding speed and laser power were adjusted to prevent the vanadium foil middle layer from completely melting. After welding, a joint consisting of a weld formed by the melting of stainless steel-copper, copper-vanadium, an incompletely melted vanadium foil and a weld formed by heat conduction of vanadium-titanium alloy was obtained.
8. The titanium steel dissimilar metal according to claim 7, characterized in that: The high-efficiency ytterbium-doped fiber laser has a laser power of 2800W-3000W and a defocus amount of 0.
9. The titanium steel dissimilar metal according to claim 8, characterized in that: The laser emission angle is 9°-12° to the material surface.
10. The titanium steel dissimilar metal according to claim 9, characterized in that: The laser welding speed is 30 mm / s. Through welding, a weld joint consisting of a stainless steel-copper weld formed by melting, and a copper-vanadium and vanadium-titanium alloy weld formed by heat conduction is formed.
Citation Information
Patent Citations
Vanadium intermediate layer-added titanium alloy-stainless steel dissimilar metal laser welding method
CN107335921A
Surfacing welding method for achieving high-chromium alloy surfacing welding on Q235 steel plate
CN110640288A
Vacuum diffusion welding method for dissimilar metals of TC4 titanium alloy and 316L stainless steel
CN111299796A
Titanium alloy and stainless steel dissimilar metal pulse laser welding method
CN111299833A
Titanium-clad steel plate, and its production method
JP2005074450A
Cited By
Dissimilar metal sheet welding method for preparing middle layer based on laser cladding
CN120587669A
A method for welding dissimilar metal thin plates based on laser cladding for preparing an intermediate layer
CN120587669B
Welding method of metal joint
CN120862001A
Heterogeneous material welding method applied to brush type sealing structure
CN121535379A
A heterogeneous material welding method applied to a brush seal structure
CN121535379B