High-strength airtight material and preparation method thereof
By increasing the preheating temperature of the polyester fiber mesh and reducing the bonding temperature, combined with the improvement of the mesh paste machine, the problems of strength and airtightness of the capstone airbag material are solved, and high-strength, flat and bubble-free high-strength airtightness is achieved Material preparation improves the airtightness and service life of the product.
Patent Information
- Application Number
- CN202411239491.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The base cloth of the existing capstone airbag material is not strong, resulting in easy damage to contact with hard stones, and the surface of the mesh woven from high-fiber yarn is uneven, affecting the bonding performance between the base cloth and the PVC film. , bubble concave holes and blasting risks may occur.
High-strength polyester fiber mesh is used for preheating and bonding. By increasing the preheating temperature of the mesh and reducing the bonding temperature, the amount of paste is controlled in combination with the new mesh paste machine to ensure the smooth surface of the material and the airtightness.
It realizes high-strength, high wear-resistant high-strength airtight material, with a flat surface without bubbles and holes, which improves the peel strength and tear strength of the product, and ensures airtightness and service life.
Smart Images

Figure CN119058206A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and particularly relates to a high-strength airtight material and a preparation method thereof. Background Art
[0002] The traditional quarrying method requires the excavation of slots that can accommodate jacks in advance. This method consumes a lot of manpower and material resources, and there is also a safety hazard of stones slipping. The top stone airbag material can easily slide into the saw seam to push the stone away due to its thin structural advantage. It is safe and labor-saving while ensuring the integrity of the stone, but the material is required to have high strength and high wear resistance. The base cloth used for the common top stone airbag materials on the market is not strong, and it is easily damaged by long-term contact and friction with hard stones. In order to improve the strength of the material and extend its service life, high-strength polyester fiber mesh is used instead of ordinary mesh. However, the mesh woven with high-density yarn is too coarse and dense, and the surface of the mesh is uneven, making it difficult for the paste to penetrate into the gaps of the mesh, affecting the bonding performance between the base cloth and the PVC film, making it easy for bubbles and concave holes to form on the surface of the material, and there is a risk of explosion during the inflation process of the subsequent product. Summary of the invention
[0003] The technical problem to be solved by the present invention is: how to prepare a high-strength airtight material with a smooth surface and good airtightness so that it can be used to prepare products with high strength requirements, such as cap stone airbags.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: to provide a method for preparing a high-strength airtight material, comprising the following steps:
[0005] S1, pasting on both sides of the high-strength mesh cloth, and then drying to obtain the pasted high-strength mesh cloth;
[0006] S2, preheating the high-strength mesh cloth, the mask and the base film, and then laminating the preheated mask and the base film on both sides of the preheated high-strength mesh cloth;
[0007] The preheating temperature of the high-strength mesh cloth is 176-192°C, and the laminating temperature is 166-178°C. The preheating temperature of the high-strength mesh cloth is greater than the laminating temperature.
[0008] The beneficial effects of the present invention are as follows: the preparation method of the high-strength airtight material provided by the present invention adopts a high mesh preheating temperature to soften the paste that has been dried and plasticized on the surface of the polyester mesh, so as to achieve the effect of not easily entrapping air when laminating and venting; at the same time, a lower laminating temperature is adopted to avoid the problem of bubbles generated by re-expansion, so that no bubbles are generated during the entire laminating process, and the peel strength and tear strength of the product are improved. The obtained high-strength airtight material has a smooth surface, no bubble concave holes, and good physical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 Shown is a photograph of a high-strength airtight material according to an example of a specific embodiment of the present invention;
[0010] Figure 2 Shown is a photograph of a high-strength airtight material of a comparative example of a specific embodiment of the present invention;
[0011] Figure 3 Shown is a schematic cross-sectional structure diagram of a mesh pasting machine according to a specific embodiment of the present invention;
[0012] Description of labels:
[0013] 1. Glue tank; 2. Glue upper roller group; 21. Glue upper roller; 3. Counter-pressure roller group; 31. Pressure roller; 4. Guide roller. DETAILED DESCRIPTION
[0014] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0015] A method for preparing a high-strength airtight material comprises the following steps:
[0016] S1, pasting on both sides of the high-strength mesh cloth, and then drying to obtain the pasted high-strength mesh cloth;
[0017] S2, preheating the high-strength mesh cloth, the mask and the base film, and then laminating the preheated mask and the base film on both sides of the preheated high-strength mesh cloth;
[0018] The preheating temperature of the high-strength mesh cloth is 176-192°C, and the laminating temperature is 166-178°C. The preheating temperature of the high-strength mesh cloth is greater than the laminating temperature.
[0019] Among them, the temperature for preheating the high-strength mesh cloth is preferably 180-190°C, more preferably 190°C. In a specific embodiment, the temperature for preheating the high-strength mesh cloth can be 178°C, 179°C, 180°C, 181°C, 182°C, 183°C, 184°C, 186°C, 187°C, or 188°C.
[0020] Among them, the bonding temperature is preferably 171-176°C, more preferably 173°C. In a specific embodiment, the bonding temperature can be 167°C, 168°C, 169°C, 170°C, 172°C, 174°C, 175°C, 177°C, or 178°C.
[0021] From the above description, it can be seen that the beneficial effect of the present invention is that, compared with the general mesh lamination, by increasing the mesh preheating temperature and reducing the laminating temperature, it is ensured that the bubbles are driven out while no new bubbles are generated, so that the problem of uneven lamination and bubbles will not occur during the entire laminating process. The obtained product has good air tightness, tear resistance and peeling performance, and has a flat surface without bubble pits.
[0022] Furthermore, the high-strength mesh is a high-strength polyester fiber mesh woven from 6000D to 12000D yarns. This yarn has the characteristics of high strength, and the tensile strength of the mesh woven therefrom can reach the requirements of 8000N / 5CM to 20000N / 5CM.
[0023] Furthermore, the amount of the glue applied is 300-350 gsm, and in specific embodiments, it can be 310 gsm, 320 gsm, 330 gsm, or 340 gsm.
[0024] From the above description, it can be seen that the inventors found that the mesh woven with high-denier yarns is too coarse and dense, and the mesh surface is uneven, and the paste is not easy to penetrate into the mesh gaps, resulting in an increase in the amount of paste, and then a large number of bubbles will remain on the surface of the mesh. When the finished product is bonded, the problem of surface bubbles and concave holes will appear, so the amount of paste needs to be reduced. Under the premise that other conditions are suitable, the amount of paste can achieve smooth bonding without bubble concave holes within the above range. A slightly higher or lower amount within the above range will not affect the bonding flatness, and can be adjusted according to the gram weight of the required product.
[0025] Further, a mesh pasting machine is used for pasting;
[0026] The mesh cloth gluing machine comprises a glue tank 1, a gluing roller group 2 and a pressing roller group 3; the gluing roller group 2 is arranged at the bottom of the glue tank 1, and the pressing roller group 3 is arranged at the notch of the glue tank 1.
[0027] Furthermore, there are two pressing roller groups 3. The pressing roller group 3 includes two pressing rollers 31 located in the same horizontal plane and axially parallel to each other; the distance between the two pressing rollers 31 is adjustable.
[0028] Furthermore, the gluing roller group 2 includes at least three gluing rollers 21 arranged side by side.
[0029] At present, it is difficult to control the amount of glue to be less than 400gsm when the commonly used glue equipment is applied to the mesh woven with high-denier yarn (6000D-12000D), resulting in that the problem of air bubbles and concave holes has been difficult to be well improved. By improving the overall structure of the glue machine, a mesh glue machine with a wider and more accurate control range for the amount of glue on the mesh is obtained, so that when the mesh glue machine is used to glue the mesh woven with high-denier yarn (6000D-12000D), the glue amount can be controlled below 400gsm, and can reach 300-350gsm, thereby overcoming the problem of surface air bubbles and concave holes.
[0030] Further, the temperature of the preheated mask and the base film is 150-170°C. Preferably, the temperature of the preheated mask is greater than the temperature of the preheated base film. In a specific embodiment, the temperature of the preheated mask and the base film can be 150°C, 151°C, 153°C, 154°C, 156°C, 157°C, 158°C, 159°C, 161°C, 162°C, 164°C, 166°C, 167°C, 168°C, 169°C.
[0031] Furthermore, the method further comprises the step: S0, ironing the high-strength mesh cloth, wherein the ironing temperature is less than 100° C., preferably 70-100° C., and more preferably 80-100° C. In a specific embodiment, the ironing temperature may be 72° C., 75° C., 81° C., 84° C., 85° C., 89° C., 90° C., 92° C., 93° C., 94° C., 95° C., 96° C., 97° C., 98° C., or 99° C.
[0032] Furthermore, the ironing is three-roll ironing. Specifically, the three-roll ironing is as follows: the mesh passes through three ironing rollers in sequence, and the temperature difference of the three ironing rollers is less than 5°C, preferably less than 2°C. The temperatures of the three ironing rollers are preferably consistent, but in the actual control process, it is difficult to control the three rollers to be exactly the same due to the influence of the surrounding environment, and the temperature difference between the three rollers needs to be minimized.
[0033] Furthermore, the drying in S1 is a two-stage drying, and the drying temperature of the first stage is lower than the drying temperature of the second stage. Preferably, the temperature difference between the drying temperature of the first stage and the drying temperature of the second stage is 4 to 10°C, more preferably 4 to 6°C. The drying temperature of the first stage and the drying temperature of the second stage are 164 to 174°C. The two-stage drying in which the temperature of the second stage is lower than that of the first stage helps to further avoid the generation of a small amount of bubbles during the drying process.
[0034] The following examples and comparative examples are all pasted with Figure 3 The mesh cloth pasting machine shown is used for pasting;
[0035] The mesh gluing machine comprises a glue tank 1, a gluing roller group 2, two sets of pressing roller groups 3 and a guide roller 4; the gluing roller group 2 is arranged at the bottom of the glue tank 1, and the pressing roller group 3 is arranged at the notch of the glue tank 1;
[0036] The two sets of pressing rollers 3 are arranged in sequence from top to bottom, and the pressing rollers 3 include two pressing rollers 31 located in the same horizontal plane and axially parallel to each other; the upper gluing roller group 2 includes three upper gluing rollers 21 arranged side by side;
[0037] When applying paste, the glue tank is filled with paste, and the paste completely covers the pressure roller 31. The mesh cloth, under the traction of the guide roller 4, passes around the three pressure rollers 31 in turn to achieve pasting, and then passes through the two groups of pressing roller groups 3 in turn. After passing through the pressing roller group 3, it passes between the two pressing rollers 31, and the excess paste squeezed by the pressing roller 31 is taken out, so as to achieve precise control of the amount of pasting.
[0038] Embodiment 1:
[0039] A method for preparing a high-strength airtight material comprises the following steps:
[0040] S0, ironing the high-strength mesh cloth, the ironing is as follows: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 86°C, 88°C, and 87°C respectively;
[0041] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 326 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 168° C., and the temperature of the second vertical dryer is 173° C.;
[0042] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller for the high-strength mesh, the temperature of the preheating roller for the face mask and the temperature of the preheating roller for the bottom film being 190°C, 165°C and 155°C;
[0043] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 171°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0044] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0045] The high-strength airtight material obtained in Example 1 is shown in Figure 1 As shown, it can be seen that the surface of the material is smooth and flat without bubbles or holes.
[0046] Embodiment 2:
[0047] A method for preparing a high-strength airtight material comprises the following steps:
[0048] S0, ironing the high-strength mesh cloth, the ironing is: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 80℃, 83℃, and 82℃ respectively;
[0049] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 349 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 170° C., and the temperature of the second vertical dryer is 174° C.;
[0050] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller of the high-strength mesh, the temperature of the face mask and the temperature of the preheating roller of the bottom film being 185°C, the temperature of the preheating roller of the face mask being 170°C and the temperature of the preheating roller of the bottom film being 163°C;
[0051] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 176°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0052] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0053] Embodiment 3:
[0054] A method for preparing a high-strength airtight material comprises the following steps:
[0055] S0, ironing the high-strength mesh cloth, the ironing is: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 90°C, 91°C, and 91°C respectively;
[0056] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 311 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 169° C., and the temperature of the second vertical dryer is 175° C.;
[0057] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with a preheating roller, the temperature of the preheating roller of the high-strength mesh, the temperature of the preheating roller of the face mask, and the temperature of the preheating roller of the bottom film are 176°C, 160°C, and 152°C;
[0058] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 173° C., laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0059] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0060] Comparative Example 1:
[0061] A method for preparing a high-strength airtight material comprises the following steps:
[0062] S0, ironing the high-strength mesh cloth, the ironing is as follows: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 112°C, 113°C, and 111°C respectively;
[0063] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 328 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 168° C., and the temperature of the second vertical dryer is 173° C.;
[0064] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller for the high-strength mesh, the temperature of the preheating roller for the face mask and the temperature of the preheating roller for the bottom film being 190°C, 165°C and 155°C;
[0065] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 171°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0066] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0067] Comparative Example 2:
[0068] A method for preparing a high-strength airtight material comprises the following steps:
[0069] S0, ironing the high-strength mesh cloth, the ironing is as follows: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 86°C, 88°C, and 87°C respectively;
[0070] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 431 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 168° C., and the temperature of the second vertical dryer is 173° C.;
[0071] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller for the high-strength mesh, the temperature of the preheating roller for the face mask and the temperature of the preheating roller for the bottom film being 190°C, 165°C and 155°C;
[0072] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 171°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0073] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0074] The high-strength airtight material obtained in Comparative Example 2 is shown in Figure 2As shown, Figure 2 The locations of the bubble cavities are circled in red, and it can be seen that there are a large number of bubble cavities on the surface of the material.
[0075] Comparative Example 3:
[0076] A method for preparing a high-strength airtight material comprises the following steps:
[0077] S0, ironing the high-strength mesh cloth, the ironing is as follows: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 86°C, 88°C, and 87°C respectively;
[0078] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 324 gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 168° C., and the temperature of the second vertical dryer is 173° C.;
[0079] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller for the high-strength mesh, the temperature of the preheating roller for the face mask and the temperature of the preheating roller for the bottom film being 190°C, 165°C and 155°C;
[0080] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 181°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0081] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0082] Comparative Example 4:
[0083] A method for preparing a high-strength airtight material comprises the following steps:
[0084] S0, ironing the high-strength mesh cloth, the ironing is as follows: let the mesh cloth pass through three ironing rollers in sequence, the temperatures of the three ironing rollers are 86°C, 88°C, and 87°C respectively;
[0085] S1. Pasting is performed on both sides of the high-strength mesh cloth, the amount of paste is 320gsm, and then drying is performed to obtain the pasted high-strength mesh cloth; the drying is specifically performed by sequentially passing through two vertical dryers, the temperature of the first vertical dryer is 168°C, and the temperature of the second vertical dryer is 173°C;
[0086] S2, preheating the high-strength mesh, the face mask and the bottom film respectively with preheating rollers, the temperature of the preheating roller for the high-strength mesh, the temperature of the preheating roller for the face mask is 160°C, the temperature of the preheating roller for the bottom film is 165°C, and the temperature of the preheating roller for the bottom film is 155°C;
[0087] S3, sending the preheated mask, the preheated high-strength mesh cloth, and the preheated base film to the laminating cylinder (hot roller) at the same time at 171°C, laminating the preheated mask and base film on both sides of the preheated high-strength mesh cloth;
[0088] S4. After embossing, cooling and rolling, a high-strength airtight material is obtained.
[0089] The pastes used in Examples 1 to 3 and Comparative Examples 1 to 4 are exactly the same.
[0090] The physical properties of the 10500D high-strength airtight materials obtained in Example 1 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 1. The test standard for thickness and gram weight is DIN EN ISO 2286-2; the test standard for tensile strength is ISO 1421:2016 Method 1, the test standard for peel strength is ISO2411, and the test standard for tear strength is GB / T 16578.
[0091] Table 1
[0092]
[0093]
[0094] It can be seen that by adopting high ironing temperature, a new gluing machine to control the amount of gluing, and combining lower lamination temperature and higher preheating temperature, the problem of air bubbles and concave holes in the finished product can be significantly improved. At the same time, the peel strength and tear strength of the product can be further improved, making it more airtight and durable.
[0095] In summary, the high-strength airtight material obtained by the preparation method provided by the present invention has a smooth surface and is free of bubbles. The physical properties include a warp tensile strength of 16200N / 5CM, a weft tensile strength of 17500N / 5CM, a surface peel strength of 505N / 5CM, a bottom peel strength of 530N / 5CM, a warp tear strength of 4618N, and a weft tear strength of 5134N, which meet the physical property indicators.
[0096] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a high-strength airtight material, It is characterized in that The following steps are involved: S1, pasting on both sides of the high-strength mesh cloth, and then drying to obtain the pasted high-strength mesh cloth; S2, preheating the high-strength mesh cloth, the mask and the base film, and then laminating the preheated mask and the base film on both sides of the preheated high-strength mesh cloth; The preheating temperature of the high-strength mesh cloth is 176-192°C, and the laminating temperature is 166-178°C. The preheating temperature of the high-strength mesh cloth is greater than the laminating temperature.
2. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The high-strength mesh cloth is a high-strength polyester fiber mesh cloth woven with 6000D-12000D yarns.
3. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The amount of the pasting in S1 is 300-350 gsm.
4. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The gluing is performed by a mesh gluing machine, which comprises a glue tank, a gluing roller group and a pressing roller group. The gluing roller group is arranged at the bottom of the glue tank, and the pressing roller group is arranged at the notch of the glue tank.
5. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The temperature of preheating the facial mask and the base film is 150-170°C.
6. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The method also includes the following steps: S0, ironing the high-strength mesh cloth, wherein the ironing temperature is less than 100°C.
7. The method for preparing the high-strength airtight material according to claim 6, It is characterized in that The ironing is three-piece ironing.
8. The method for preparing the high-strength airtight material according to claim 1, It is characterized in that The drying in S1 is a two-stage drying, and the drying temperature of the first stage is lower than the drying temperature of the second stage.
9. The method for preparing the high-strength airtight material according to claim 8, It is characterized in that The temperature difference between the drying temperature of the first stage and the drying temperature of the second stage is 5-10°C.
10. A high-strength airtight material prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Production process for high-strength dacron laminated film construction material
CN101509203A
Novel waterproof membrane material with patterns and preparation method thereof
CN102632671A
Production process of air cushion
CN102848688A
PVC composite material for biogas digester and preparation method of PVC composite material
CN104553171A
Preparation method of reinforced composite spatial mesh material
CN107310238A
Cited By
Preparation method of polyvinyl chloride tarpaulin with flat surface
CN120363484A