Long-life tundish cover castable

By optimizing the material ratio and treatment technology of the castable material of the intermediate bag cover, an efficient protective oxide layer and dense structure are formed, which solves the problems of insufficient high temperature resistance, poor thermal shock resistance and weak corrosion resistance, and significantly extends the use Lifespan and cost reduction, achieving efficient and environmentally friendly construction performance.

CN119059803APending Publication Date: 2024-12-03SHANGHAI LIER REFRACTORY MATERIAL +1

Patent Information

Application Number
CN202411490418.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The castable material with intermediate bag covers has insufficient high temperature resistance, poor thermal shock resistance, weak corrosion resistance and poor construction performance, resulting in short service life and high cost.

Method used

Use specific ratios of alumina, mullite, azure, silicon carbide, ferrosilicon powder, composite bonding agent, calcium silicate, aluminum silicate fiber, waste electromelt bricks and alumina powder and other materials, through thermal oxidation Treatment and particle size optimization form an efficient protective oxide layer and dense structure, improving oxidation resistance, corrosion resistance and construction performance.

Benefits of technology

It significantly extends the service life of the intermediate bag cap castable, improves oxidation resistance, corrosion resistance, thermal stability and construction performance, reduces costs, is suitable for use in high temperature environments, and realizes the dual value of environmental protection and economic benefits. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005099886620000161
    Figure BDA0005099886620000161
  • Figure BDA0005099886620000171
    Figure BDA0005099886620000171
Patent Text Reader

Abstract

The invention discloses a long-life tundish cover castable, and relates to the technical field of tundish refractory materials. The long-life tundish cover castable is prepared from the following raw material components in percentage by mass: 5 to 7 percent of 15 to 8 mm alumina, 12 to 14 percent of 8 to 5 mm alumina, 12 to 14 percent of 5 to 3 mm alumina, 22 to 24 percent of 3 to 1 mm alumina, 8 to 10 percent of 1 to 0 mm alumina, 13 to 15 percent of 200-mesh alumina, 1 to 2 percent of mullite, 3.5 to 4.5 percent of kyanite, 1.5 to 2.5 percent of silicon carbide, 0.2 to 0.3 percent of silicon iron powder, 3 to 4 percent of composite binding agent, 0.6 to 0.8 percent of calcium silicate and 0.1 to 0.5 percent of alumina silicate fiber. The invention discloses a long-service-life tundish cover castable which comprises the following components in percentage by weight: 0.2% of waste fused bricks, 0.5-0.7% of aluminum oxide micro powder, 0.08-0.1% of sodium tripolyphosphate, 2.5-3% of silica fume, 0.02-0.03% of organic fibers, 1% of steel fibers and 3-4% of high-alumina cement. Compared with a traditional process, the overall performance of the tundish cover castable is remarkably improved, and the long-service-life tundish cover castable is more suitable for being used in a high-temperature environment; the breaking strength and the compression strength of the castable are effectively enhanced, the service life of the castable is prolonged, and meanwhile, the dual values of environmental protection and economic benefits are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tundish refractory materials, and in particular relates to a long-life tundish cover castable. Background Art

[0002] The steel industry is one of the pillar industries of the national economy, and the development of continuous casting technology has greatly improved production efficiency and product quality. In the continuous casting process, the tundish plays a vital role as a transition container for molten steel refining and distribution. It can not only regulate the temperature and flow of molten steel and remove impurities, but also control the purity and stability of molten steel, which directly affects the quality and performance of the final product. Therefore, the refractory material of the tundish, especially the performance of the tundish cover, has become one of the key factors to ensure the efficient and stable operation of the continuous casting machine.

[0003] The main function of the tundish cover is to provide insulation for the tundish during the continuous casting process, prevent excessive heat loss of the molten steel, and protect the molten steel from oxygen erosion in the air to avoid the production of secondary oxides. However, since the tundish needs to withstand extreme temperature conditions (up to 1600°C or above) and frequent hot and cold cycles during operation, this poses a severe challenge to the refractory materials of the tundish cover. The traditional tundish cover castable has the following problems: First, the high temperature resistance is insufficient, resulting in a short service life; second, the thermal shock resistance is poor, and it is easy to crack and peel off when the temperature changes sharply; third, the corrosion resistance is weak, and when facing the corrosive medium in the molten steel, chemical reactions are prone to occur, affecting the quality of the molten steel; fourth, the construction performance is poor, and it is difficult to meet the needs of rapid on-site repairs, which places extremely high demands on the high temperature resistance and thermal shock resistance of the castable.

[0004] At present, the tundish cover castable is mainly made of high-aluminum, magnesium or magnesium-aluminum composite materials, which are prepared by adding auxiliary materials such as binders, expanders and antioxidants. Although these materials can meet the use requirements to a certain extent, they generally have the problems of short service life and high cost. Summary of the invention

[0005] In view of the problems that the existing long-life tundish cover castable has insufficient high temperature resistance, poor thermal shock resistance, weak erosion resistance and poor construction performance, the present invention provides a long-life tundish cover castable, which overcomes the defects of traditional tundish cover castables, can significantly improve the construction performance, erosion resistance and strength of the tundish cover castable, and effectively prolong the service life of the long-life tundish cover castable.

[0006] The solution adopted by the present invention to solve the technical problem is: a long-life tundish cover castable, wherein the mass percentage of each raw material component in the long-life tundish cover castable is: 15-8mm alumina is 5-7%, 8-5mm alumina is 12-14%, 5-3mm alumina is 12-14%, 3-1mm alumina is 22-24%, 1-0mm alumina is 8-10%, 200 mesh alumina is 13-15%, mullite is 1-2%, blue crystal is 1% Stone is 3.5-4.5%, silicon carbide is 1.5-2.5%, ferrosilicon powder is 0.2-0.3%, composite binder is 3-4%, calcium silicate is 0.6-0.8%, aluminum silicate fiber is 0.1-0.2%, waste fused brick is 0.5-0.7%, alumina powder is 2.5-3%, sodium tripolyphosphate is 0.08-0.1%, silica fume is 2.5-3%, organic fiber is 0.02-0.03%, steel fiber is 1%, and high alumina cement is 3-4%.

[0007] Furthermore, the long-life tundish cover castable contains 6% 15-8mm alumina, 12.5% ​​8-5mm alumina, 13% 5-3mm alumina, 22.8% 3-1mm alumina, 9% 1-0mm alumina, 13.9% 200-mesh alumina, 1.5% mullite, 4% kyanite, 1.9% silicon carbide, 0.3% ferrosilicon powder, 3.4% composite binder, 0.75% calcium silicate, 0.14% aluminum silicate fiber, 0.6% waste fused brick, 2.8% alumina powder, 0.09% sodium tripolyphosphate, 2.8% silica ash, 0.02% organic fiber, 1% steel fiber, and 3.5% high-alumina cement.

[0008] Furthermore, the Al2O3 content in the 15-8mm bauxite is ≥80%; the Al2O3 content in the 8-5mm bauxite is ≥80%; the Al2O3 content in the 5-3mm bauxite is ≥85%; the Al2O3 content in the 3-1mm bauxite is ≥85%; the Al2O3 content in the 1-0mm bauxite is ≥87%; the Al2O3 content in the 200-mesh bauxite is ≥87%; the mullite is 200-mesh sintered mullite; the kyanite particle size is 100 mesh; the calcium silicate particle size is 1250 mesh, and the melting point is ≥1500°C; the sodium tripolyphosphate is industrial grade; the SiO2 content in the silica ash is ≥95%; and the Al2O3 content in the high-alumina cement is ≥71%.

[0009] Furthermore, the mass percentages of the raw material components in the composite binder are: polyvinyl alcohol is 12%, silica sol is 88%, and the effective ingredient content of silica sol is 30%.

[0010] Furthermore, the mass percentage of each raw material component in the silicon carbide is: 60% of silicon carbide with a particle size of 80 meshes, and 40% of silicon carbide with a particle size of 400 meshes.

[0011] Furthermore, the mass percentages of the raw material components in the alumina fine powder are as follows: 60% of the alumina with a particle size of 1 μm, and 40% of the alumina with a particle size of 3 μm.

[0012] Furthermore, the ferrosilicon powder has a particle size of 200 meshes and its surface is thermally oxidized.

[0013] Furthermore, the aluminum silicate fiber has a length of 3-20 mm and a diameter of 1-6 μm.

[0014] Furthermore, the waste fused bricks are used AZS fused bricks with a particle size of 600 mesh.

[0015] Furthermore, the castable is suitable for T-type tundishes with 5 streams or more.

[0016] The present invention selects ferrosilicon powder, and utilizes thermal oxidation treatment to change the properties of the surface of the ferrosilicon powder, making it more suitable as an additive for the castable of the present invention. The positive effects of thermal oxidation treatment on the ferrosilicon powder are as follows: first, the iron and silicon in the ferrosilicon powder can form a mixed oxide layer composed of Fe2O3 and SiO2 with high melting point and good chemical stability in a high-temperature oxidizing atmosphere, which can form a dense barrier layer, effectively protecting the internal ferrosilicon from further erosion, and significantly improving the castable's corrosion resistance to molten metal and slag. The formed mixed oxide layer can also promote chemical interaction with other components in the castable, and can effectively enhance the interface bonding force between the ferrosilicon powder and the castable matrix; secondly, the ferrosilicon powder Harmful volatiles, such as silane, may be released at high temperatures. Thermal oxidation treatment can consume highly active silicon, reduce the generation of such volatiles, and avoid pollution to the castable and the surrounding environment. At the same time, thermal oxidation treatment improves the thermal and chemical stability of ferrosilicon powder, making it less likely to decompose or undergo adverse chemical reactions in the high-temperature working environment of the castable. In addition, the formation of an oxide layer also helps control the volume expansion of the castable during heating and cooling, reducing the risk of cracks and spalling, thereby extending the service life of the castable. Surface-treated ferrosilicon powder has better dispersibility and fluidity, which helps to distribute it more evenly when stirring the castable, thereby improving the overall performance of the castable. Therefore, thermal oxidation treatment not only changes the surface properties of ferrosilicon powder, but also improves the oxidation resistance, corrosion resistance, thermal stability, structural strength and construction performance of the tundish cover castable, thereby significantly extending the service life of the castable.

[0017] The present invention adopts a composite binder, which is composed of polyvinyl alcohol and silica sol, and the mass percentage of the raw material components is: polyvinyl alcohol is 12%, and silica sol is 88%. The performance of the castable can be significantly improved, and the synergistic effect of the composite binder can be used to produce the following effects: first, polyvinyl alcohol and silica sol are used in combination, polyvinyl alcohol provides adhesion and plasticity at low temperatures, and silica sol provides strength and stability at high temperatures, so that the castable has both good construction performance and excellent high-temperature performance; secondly, the synergistic effect of the two helps to control the shrinkage of the castable during the hardening process, reduce the risk of cracking, and thus improve the integrity and service life of the castable; finally, polyvinyl alcohol and silica sol are used in combination to comprehensively improve the strength, corrosion resistance, thermal shock resistance and construction performance of the castable, so that the castable is more suitable for use in harsh high-temperature environments, thereby achieving a tundish cover castable with higher strength, better thermal stability and longer service life.

[0018] The present invention selects 1250 mesh calcium silicate, and its functions are mainly reflected in: first, the 1250 mesh calcium silicate fine powder has a very fine particle size, which can fill the tiny pores in the castable, improve the density of the castable, reduce the porosity, and thus improve the material's anti-permeability and anti-erosion properties; second, the thermal expansion coefficient of calcium silicate is relatively low, which helps to reduce the thermal stress of the castable during the thermal cycle, reduce the cracking and spalling caused by thermal shock, and improve the thermal stability of the castable; in addition, at high temperatures, calcium silicate can react with other components in the castable to form a glass phase or crystalline phase with a high melting point and low permeability, such as mullite, to form a protective layer on the surface of the castable to resist the erosion of slag and molten steel; fine-grained calcium silicate can be at high temperatures Promoting the sintering process helps to form a denser microstructure and improve the mechanical strength and high-temperature performance of the castable. At the same time, calcium silicate can reduce the sintering temperature of the castable at high temperature, promote the formation of liquid phase, and help densify the castable structure, thereby improving the high-temperature strength and wear resistance of the material. Fine-grained calcium silicate can improve the fluidity of the castable, making it easier to apply or pour during construction, and is also beneficial to the release of water in the castable during the hardening process and reducing the formation of pores. Finally, as an environmentally friendly material, the production and use process of calcium silicate is relatively clean and does not produce harmful substances, which meets the needs of modern industry for environmentally friendly materials. The selection of 1250 mesh calcium silicate is based on a balance between comprehensive performance and cost-effectiveness.

[0019] The present invention adopts aluminum silicate fiber, and its main functions are as follows: first, the aluminum silicate fiber forms a three-dimensional network structure in the castable, which can effectively disperse stress, improve the tensile strength and toughness of the castable, and reduce the breakage caused by external force. The fiber forms a continuous network in the castable, which can block the penetration of slag and molten steel, reduce the direct contact of the corrosive medium with the castable matrix, and thus improve the corrosion resistance; secondly, the addition of aluminum silicate fiber can slow down the thermal expansion of the castable when the temperature changes, and there is a small gap between the fiber and the matrix material, which can absorb part of the thermal stress and reduce the cracking caused by thermal shock; Aluminum fiber can occupy space during the hardening process of castables, prevent the formation of pores, increase the density of castables, reduce porosity, and thus improve overall performance; at the same time, aluminum silicate fiber has good structural stability at high temperatures, can maintain its shape unchanged, continue to provide reinforcement for castables, and improve the high-temperature strength and wear resistance of castables; aluminum silicate fiber is slender, which can improve the fluidity of castables, making it easier to spread and shape during construction, and improve construction efficiency; in addition, aluminum silicate fiber has a low thermal conductivity, which can reduce the heat conduction of castables, improve its thermal insulation performance, and reduce heat loss. In summary, aluminum silicate fiber can significantly improve the tensile strength, thermal shock resistance, erosion resistance, structural density, high-temperature performance and construction performance of castables, and through fiber reinforcement, thermal expansion buffering, physical barriers, structural densification, thermal insulation and other mechanisms, comprehensively improve the comprehensive performance of castables and extend their service life.

[0020] The present invention adds used AZS fused bricks to improve the performance of the castable, and its effects are mainly reflected as follows: first, AZS fused bricks contain a high proportion of Al2O3 and ZrO2, and these components have strong resistance to slag and molten steel at high temperatures; AZS fused bricks have a low thermal expansion coefficient, which can improve the thermal expansion characteristics of the castable, reduce the thermal stress caused by temperature changes, and thus significantly improve the thermal shock resistance of the castable; secondly, AZS fused bricks can form stable crystalline phases such as corundum, zircon, etc. at high temperatures, and these crystalline phases can significantly improve the structural stability and strength of the castable at high temperatures; at the same time, the addition of waste AZS fused bricks can improve the particle grading of the castable, so that the castable has better fluidity during construction, while reducing the formation of pores and improving the density of the castable; in addition, the use of waste AZS fused bricks can realize the recycling of resources, reduce the cost of castables, and reduce the problem of waste disposal, which is in line with the concept of sustainable development. In summary, the addition of waste fused bricks can significantly improve the comprehensive performance of the tundish cover castable, extend its service life, and at the same time promote the recycling of resources, reflecting the dual value of environmental protection and economic benefits.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention uses ferrosilicon powder to improve the oxidation resistance, corrosion resistance, thermal stability, structural strength and construction performance of the castable, and significantly prolongs the service life of the castable. The specific effects include forming a protective oxide layer, improving interface bonding, reducing harmful volatiles, controlling volume expansion, and improving dispersibility and fluidity;

[0023] 2. The present invention adds a composite binder (polyvinyl alcohol and silica sol) to enhance the construction performance and high temperature performance of the castable, reduce the risk of shrinkage and cracking during the hardening process, and improve the strength, corrosion resistance, and thermal shock resistance of the castable, making it more suitable for use in harsh high temperature environments;

[0024] 3. The present invention adopts 1250 mesh calcium silicate, which improves the density, permeability resistance, corrosion resistance, thermal stability, mechanical strength and high temperature performance of the castable, while improving the construction performance, being environmentally friendly, and balancing the comprehensive performance and cost-effectiveness;

[0025] 4. The present invention uses aluminum silicate fiber to significantly improve the tensile strength, thermal shock resistance, corrosion resistance, structural density, high temperature performance and construction performance of the castable, and improves the comprehensive performance of the castable through multiple mechanisms;

[0026] 5. The present invention introduces waste AZS fused bricks, which improves the thermal shock resistance, structural stability and strength of the castable at high temperatures, improves particle grading and fluidity, promotes the recycling of resources, reduces costs, and complies with the concept of sustainable development.

[0027] In summary, compared with the traditional process, the tundish cover castable of the present invention significantly improves the overall performance of the tundish cover castable, including oxidation resistance, corrosion resistance, thermal stability, thermal shock resistance, structural strength and construction performance, through material selection and ratio optimization, and is more suitable for use in high temperature environments. The flexural strength and compressive strength of the castable are also effectively enhanced, which extends the service life of the castable, while achieving the dual value of environmental protection and economic benefits. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] The present invention provides a technical solution for a long-life tundish cover castable:

[0030] A long-life tundish cover castable, 15-8mm alumina is 5-7%, 8-5mm alumina is 12-14%, 5-3mm alumina is 12-14%, 3-1mm alumina is 22-24%, 1-0mm alumina is 8-10%, 200 mesh alumina is 13-15%, mullite is 1-2%, kyanite is 3.5-4.5%, silicon carbide is 1.5-2.5 %, ferrosilicon powder is 0.2-0.3%, composite binder is 3-4%, calcium silicate is 0.6-0.8%, aluminum silicate fiber is 0.1-0.2%, waste fused brick is 0.5-0.7%, alumina powder is 2.5-3%, sodium tripolyphosphate is 0.08-0.1%, silica fume is 2.5-3%, organic fiber is 0.02-0.03%, steel fiber is 1%, and high alumina cement is 3-4%.

[0031] As a preferred embodiment of the present invention, the long-life tundish cover castable contains 6% 15-8mm alumina, 12.5% ​​8-5mm alumina, 13% 5-3mm alumina, 22.8% 3-1mm alumina, 9% 1-0mm alumina, 13.9% 200-mesh alumina, 1.5% mullite, 4% kyanite, 1.9% silicon carbide, 0.3% ferrosilicon powder, 3.4% composite binder, 0.75% calcium silicate, 0.14% aluminum silicate fiber, 0.6% waste fused brick, 2.8% alumina powder, 0.09% sodium tripolyphosphate, 2.8% silica ash, 0.02% organic fiber, 1% steel fiber and 3.5% high-alumina cement.

[0032] As a preferred embodiment of the present invention, the Al2O3 content in the 15-8mm bauxite is ≥80%; the Al2O3 content in the 8-5mm bauxite is ≥80%; the Al2O3 content in the 5-3mm bauxite is ≥85%; the Al2O3 content in the 3-1mm bauxite is ≥85%; the Al2O3 content in the 1-0mm bauxite is ≥87%; the Al2O3 content in the 200-mesh bauxite is ≥87%; the mullite is 200-mesh sintered mullite; the kyanite particle size is 100 mesh; the calcium silicate particle size is 1250 mesh, and the melting point is ≥1500°C; the sodium tripolyphosphate is industrial grade; the SiO2 content in the silica ash is ≥95%; the Al2O3 content in the high-alumina cement is ≥71%.

[0033] The present invention adopts a combination of large-particle alumina with a relatively low alumina content and fine-powder alumina with a relatively high alumina content, which can optimize the performance of the covered castable. The large-particle alumina provides structural support and fluidity, while the fine-powder alumina enhances the density and chemical stability of the material. This alumina particle size combination enables the castable to withstand high temperature and mechanical loads and maintain good physical and chemical properties in a high-temperature environment. Moreover, compared with some other more expensive refractory materials, alumina has a lower cost and can provide sufficient performance at the same time, balancing cost and performance, and achieving the dual goals of economic benefit and use effect.

[0034] The present invention selects sintered mullite for addition because sintered mullite has excellent thermal stability, chemical stability, high temperature strength, corrosion resistance and good bonding performance, and can significantly improve the refractory performance, thermal stability and chemical stability of the ladle cover castable, thereby ensuring the safety and economy of the continuous casting process; since alumina is susceptible to thermal shock damage due to uneven thermal expansion, the present invention can significantly improve the thermal shock resistance of the castable by adding 200-mesh mullite and 100-mesh kyanite, by adding mullite and kyanite to utilize their synergistic effect, which not only improves the thermal shock resistance and corrosion resistance of the castable, but also enhances its high-temperature structural strength and construction performance, which is of great significance for extending the service life of the tundish cover and improving the stability and efficiency of the continuous casting process;

[0035] The present invention adopts industrial-grade sodium tripolyphosphate, which can significantly improve the wear resistance, thermal stability, thermal shock resistance and erosion resistance of the castable, and at the same time effectively prolong the service life of the castable by promoting sintering and improving construction performance, ensuring that it maintains excellent performance in a high-temperature environment, thereby improving the overall durability and work efficiency of the tundish;

[0036] The present invention adopts silica fume with high content of SiO2, which can react well with other components in the castable to form a stable silicate network structure, which not only improves the mechanical strength and wear resistance of the castable, but also significantly enhances its ability to resist alkali erosion and sulfate erosion. In addition, the fine particles of silica fume can effectively fill the tiny pores in the castable, reduce the porosity, and thus improve the density and impermeability of the castable. In a high temperature environment, this castable exhibits excellent thermal stability and thermal shock resistance, ensuring the structural integrity and service life of the tundish cover during repeated heating and cooling.

[0037] The present invention adopts 1250 mesh calcium silicate, because its fine particle size can improve the density and permeability resistance of the castable, the low thermal expansion coefficient enhances the thermal stability, promotes sintering at high temperature to form a protective layer, improves the mechanical strength and high temperature performance, and improves the fluidity and reduces the sintering temperature, enhances the wear resistance, and meets the environmental protection requirements. It is a preferred material based on the balance of performance and cost-effectiveness; the melting point of calcium silicate is as high as 1500°C or more, which can improve the refractory performance of the castable and ensure the stability and durability of the cover in a high temperature environment;

[0038] The present invention selects high-alumina cement with high Al2O3 content, which can improve the high-temperature resistance of the overall material, making it more suitable for use in high-temperature environments, and can also enhance the overall strength and crack resistance of the castable to a certain extent.

[0039] As a preferred embodiment of the present invention, the mass percentages of the raw material components in the composite binder are: polyvinyl alcohol is 12%, silica sol is 88%, and the effective ingredient content of silica sol is 30%.

[0040] The present invention adopts a composite binder, which is composed of polyvinyl alcohol and silica sol. The mass percentage of the raw material components is: polyvinyl alcohol is 12%, and silica sol is 88%. The performance of the castable can be significantly improved. The synergistic effect of the composite binder can produce the following effects: first, polyvinyl alcohol and silica sol are used in combination, polyvinyl alcohol provides adhesion and plasticity at low temperatures, and silica sol provides strength and stability at high temperatures, so that the castable has both good construction performance and excellent high-temperature performance; secondly, the synergistic effect of the two helps to control the shrinkage of the castable during the hardening process and reduce the risk of cracking. , thereby improving the integrity and service life of the castable; at the same time, the effective ingredient content of silica sol is 30%, and the effective ingredient in silica sol is silicon dioxide, which can form an interpenetrating network structure with polyvinyl alcohol, enhance the mechanical strength and bonding force of the castable, and enable the cover to maintain structural integrity at high temperature and during use; finally, the combination of polyvinyl alcohol and silica sol can comprehensively improve the strength, corrosion resistance, thermal shock resistance and construction performance of the castable, making the castable more suitable for use in harsh high temperature environments, thereby achieving higher strength, better thermal stability and longer service life of the intermediate ladle cover castable.

[0041] As a preferred embodiment of the present invention, the mass percentages of the raw material components in the silicon carbide are: 60% of the silicon carbide with a particle size of 80 meshes, and 40% of the silicon carbide with a particle size of 400 meshes.

[0042] The silicon carbide selected in the present invention adopts a mixture of silicon carbide of different particle sizes, which can bring the following positive effects: first, by introducing high-hardness silicon carbide, especially 80-mesh coarse-grained silicon carbide, the wear resistance of the castable is significantly enhanced, and the erosion of molten steel and slag is effectively resisted; secondly, the high thermal conductivity and low thermal expansion coefficient of silicon carbide effectively improve the thermal shock resistance of the castable, reduce the thermal stress caused by temperature difference, and avoid material cracking; thirdly, the fine filling effect of 400-mesh fine-grained silicon carbide improves the density and structural strength of the castable; in addition, compounds such as mullite generated by the reaction of silicon carbide with other components at high temperature promote the sintering of the material and enhance the overall structure; the mixed use of silicon carbide of different particle sizes also optimizes the fluidity of the castable and improves the construction performance; at the same time, the chemical stability of silicon carbide at high temperature enhances the corrosion resistance of the castable; finally, through the optimization of particle grading, a balance between the density, wear resistance and thermal shock resistance of the castable is achieved, and the material performance is comprehensively improved.

[0043] As a preferred embodiment of the present invention, the aluminum oxide with a particle size of 1 μm accounts for 60%, and the aluminum oxide with a particle size of 3 μm accounts for 40%.

[0044] The invention adds alumina powder, the particle size of which is a mixture of 1 μm and 3 μm, which can significantly improve the performance of the castable, and its effects are mainly reflected in: first, the fine particle size of the alumina powder can effectively fill the tiny pores in the castable, reduce the porosity, thereby improving the density, and then reducing the permeability of the castable and enhancing its corrosion resistance; second, the fine particle size alumina powder is conducive to the formation of liquid phase at high temperature, accelerates the sintering process, and makes the castable structure denser and stronger; third, the stable crystal structure formed by the alumina powder at high temperature, such as corundum, significantly improves the high temperature strength and wear resistance of the castable; in addition, the fine particle size alumina powder The similar thermal expansion coefficient of aluminum powder and other components of castable reduces the internal stress caused by thermal expansion and contraction, and improves the thermal shock resistance of castable. Furthermore, the excellent chemical stability of alumina powder effectively resists the erosion of molten steel and slag. At the same time, fine-grained alumina powder improves the fluidity of castable, facilitates construction spreading and molding, and improves construction efficiency. Furthermore, the mixed use of alumina powders of different particle sizes optimizes the particle grading, balances the density and construction performance of the material, and further improves the overall performance. Finally, fine alumina powder acts as a reinforcing phase to enhance the mechanical strength of the castable, especially the strength performance under high temperature conditions.

[0045] As a preferred embodiment of the present invention, the ferrosilicon powder has a particle size of 200 meshes and its surface is thermally oxidized.

[0046] The present invention uses ferrosilicon powder that has been subjected to thermal oxidation treatment to change its surface properties and improve its performance as a castable additive. The treated ferrosilicon powder can form a dense Fe2O3 and SiO2 mixed oxide layer, thereby enhancing corrosion resistance and interface bonding strength, reducing harmful volatiles, improving thermal stability and chemical stability, controlling volume expansion, reducing the risk of cracks, and effectively improving dispersibility and fluidity, thereby comprehensively improving the castable's oxidation resistance, corrosion resistance, thermal stability, structural strength and construction performance, and significantly extending the castable's service life.

[0047] As a preferred embodiment of the present invention, the aluminum silicate fiber has a length of 3-20 mm and a diameter of 1-6 μm.

[0048] The aluminum silicate fibers of the above length and diameter are selected in the present invention, which has the following effects: first, aluminum silicate fibers of appropriate length can form an effective three-dimensional network structure in the castable, enhance the cohesion of the material, and thus improve the mechanical properties of the castable, such as compression and tension; second, the fine fibers can more effectively block the transfer of heat, so that the castable can better maintain the stability of its internal temperature under high temperature environment, thereby extending the service life; third, the appropriate fiber size helps the fibers to be evenly distributed in the castable, avoid agglomeration and sedimentation, thereby ensuring that the overall performance of the castable is uniform and consistent, and also has good chemical stability and thermal stability. They can resist the erosion of a variety of chemical substances and maintain stable physical and chemical properties at high temperatures; at the same time, the uniform distribution of fibers also helps to reduce bubbles and pores during the construction process, and improves the density and quality of the castable.

[0049] As a preferred embodiment of the present invention, the waste fused bricks are used AZS fused bricks with a particle size of 600 mesh, and the castable is suitable for T-type tundishes with 5 streams or more.

[0050] Specific implementation cases:

[0051] A specific embodiment of a long-life tundish cover castable of the present invention is provided below.

[0052] Embodiment 1:

[0053] The present embodiment provides a long-life tundish cover castable, and the long-life tundish cover castable has the following components in percentage by mass: 6% of 15-8mm alumina, 12.5% ​​of 8-5mm alumina, 13% of 5-3mm alumina, 22.8% of 3-1mm alumina, 9% of 1-0mm alumina, 13.9% of 200-mesh alumina, 1.5% of mullite, 4% of kyanite, 1.9% of silicon carbide, 0.3% of ferrosilicon powder, 3.4% of composite binder, 0.75% of calcium silicate, 0.14% of aluminum silicate fiber, 0.6% of waste fused brick, 2.8% of alumina powder, 0.09% of sodium tripolyphosphate, 2.8% of silica ash, 0.02% of organic fiber, 1% of steel fiber, and 3.5% of high-alumina cement.

[0054] Embodiment 2:

[0055] The present embodiment provides a long-life tundish cover castable, and the percentage of each component of the long-life tundish cover castable is as follows: 6.4% of 15-8mm alumina, 13.6% of 8-5mm alumina, 14% of 5-3mm alumina, 23% of 3-1mm alumina, 8% of 1-0mm alumina, 13.6% of 200-mesh alumina, 1.7% of mullite, 3.7% of kyanite, 1.5% of silicon carbide, 0.2% of ferrosilicon powder, 3.1% of composite binder, 0.8% of calcium silicate, 0.19% of aluminum silicate fiber, 0.7% of waste fused brick, 2.5% of alumina powder, 0.08% of sodium tripolyphosphate, 2.6% of silica ash, 0.03% of organic fiber, 1% of steel fiber, and 3.3% of high-alumina cement.

[0056] Embodiment 3:

[0057] The present embodiment provides a long-life tundish cover castable, and the long-life tundish cover castable has the following components in percentage by mass: 7% of 15-8mm alumina, 12.3% of 8-5mm alumina, 13.7% of 5-3mm alumina, 22% of 3-1mm alumina, 8.7% of 1-0mm alumina, 13.3% of 200-mesh alumina, 1% of mullite, 3.6% of kyanite, 2.3% of silicon carbide, 0.2% of ferrosilicon powder, 4% of composite binder, 0.68% of calcium silicate, 0.1% of aluminum silicate fiber, 0.6% of waste fused brick, 3% of alumina powder, 0.1% of sodium tripolyphosphate, 2.7% of silica ash, 0.02% of organic fiber, 1% of steel fiber, and 3.7% of high-alumina cement.

[0058] Embodiment 4:

[0059] The present embodiment provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows by mass percentage: 5.3% of 15-8mm alumina, 12% of 8-5mm alumina, 12% of 5-3mm alumina, 23.4% of 3-1mm alumina, 10% of 1-0mm alumina, 15% of 200-mesh alumina, 1.4% of mullite, 4.5% of kyanite, 1.7% of silicon carbide, 0.3% of ferrosilicon powder, 3.3% of composite binder, 0.68% of calcium silicate, 0.2% of aluminum silicate fiber, 0.5% of waste fused bricks, 2.7% of alumina powder, 0.09% of sodium tripolyphosphate, 2.8% of silica ash, 0.03% of organic fiber, 1% of steel fiber, and 3.1% of high-alumina cement.

[0060] Embodiment 5:

[0061] The present embodiment provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows: 5% of 15-8mm alumina, 14% of 8-5mm alumina, 12.3% of 5-3mm alumina, 24% of 3-1mm alumina, 8.8% of 1-0mm alumina, 14.2% of 200-mesh alumina, 1.2% of mullite, 3.5% of kyanite, 1.6% of silicon carbide, 0.3% of ferrosilicon powder, 3% of composite binder, 0.6% of calcium silicate, 0.1% of aluminum silicate fiber, 0.7% of waste fused bricks, 2.6% of alumina powder, 0.08% of sodium tripolyphosphate, 3% of silica ash, 0.02% of organic fiber, 1% of steel fiber, and 4% of high-alumina cement.

[0062] Embodiment 6:

[0063] The present embodiment provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows by mass percentage: 15-8mm alumina is 5.9%, 8-5mm alumina is 13%, 5-3mm alumina is 13.1%, 3-1mm alumina is 22.2%, 1-0mm alumina is 9.6%, 200-mesh alumina is 13%, mullite is 2%, kyanite is 3.9%, silicon carbide is 2.5%, ferrosilicon powder is 0.2%, composite binder is 3.7%, calcium silicate is 0.78%, aluminum silicate fiber is 0.2%, waste fused brick is 0.5%, alumina powder is 2.8%, sodium tripolyphosphate is 0.1%, silica ash is 2.5%, organic fiber is 0.02%, steel fiber is 1%, and high alumina cement is 3%.

[0064] Comparative Example 1:

[0065] The present comparative example provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows by mass percentage: 6.59% of 15-8mm alumina, 13.6% of 8-5mm alumina, 14% of 5-3mm alumina, 23% of 3-1mm alumina, 8% of 1-0mm alumina, 13.6% of 200-mesh alumina, 1.7% of mullite, 3.7% of kyanite, 1.5% of silicon carbide, 0.2% of ferrosilicon powder, 3.1% of composite binder, 0.8% of calcium silicate, 0.7% of waste fused bricks, 2.5% of alumina powder, 0.08% of sodium tripolyphosphate, 2.6% of silica ash, 0.03% of organic fiber, 1% of steel fiber, and 3.3% of high-alumina cement. The present comparative example does not contain aluminum silicate fiber.

[0066] Comparative Example 2:

[0067] The comparative example provides a long-life tundish cover castable, wherein the long-life tundish cover castable comprises, by mass percentage, 7% of 15-8mm alumina, 12.3% of 8-5mm alumina, 13.7% of 5-3mm alumina, 22% of 3-1mm alumina, 8.7% of 1-0mm alumina, 13.3% of 200-mesh alumina, and 1% of mullite. , kyanite is 3.6%, silicon carbide is 2.3%, ferrosilicon powder is 0.2%, composite binder is 4%, calcium silicate is 0.68%, aluminum silicate fiber is 0.1%, waste fused brick is 0.6%, alumina powder is 3%, sodium tripolyphosphate is 0.1%, silica ash is 2.7%, organic fiber is 0.02%, steel fiber is 1%, and high alumina cement is 3.7%. In this comparative example, the composite binder is all silica sol.

[0068] Comparative Example 3:

[0069] The present comparative example provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows by mass percentage: 5.6% of 15-8mm alumina, 12% of 8-5mm alumina, 12% of 5-3mm alumina, 23.4% of 3-1mm alumina, 10% of 1-0mm alumina, 15% of 200-mesh alumina, 1.4% of mullite, 4.5% of kyanite, 1.7% of silicon carbide, 3.3% of composite binder, 0.68% of calcium silicate, 0.2% of aluminum silicate fiber, 0.5% of waste fused bricks, 2.7% of alumina powder, 0.09% of sodium tripolyphosphate, 2.8% of silica ash, 0.03% of organic fiber, 1% of steel fiber, and 3.1% of high-alumina cement. The present comparative example does not contain ferrosilicon powder.

[0070] Comparative Example 4:

[0071] The present comparative example provides a long-life tundish cover castable, and the percentages of the components of the long-life tundish cover castable are as follows by mass percentage: 15-8mm alumina is 5.6%, 8-5mm alumina is 14%, 5-3mm alumina is 12.3%, 3-1mm alumina is 24%, 1-0mm alumina is 8.8%, 200-mesh alumina is 14.2%, mullite is 1.2%, kyanite is 3.5%, silicon carbide is 1.6%, ferrosilicon powder is 0.3%, composite binder is 3%, aluminum silicate fiber is 0.1%, waste fused brick is 0.7%, alumina powder is 2.6%, sodium tripolyphosphate is 0.08%, silica ash is 3%, organic fiber is 0.02%, steel fiber is 1%, and high alumina cement is 4%. The present comparative example does not contain calcium silicate.

[0072] The present invention prepares samples of a long-life tundish cover castable of Examples 1 to 6 and Comparative Examples 1 to 4 according to GB / T 4513.5-2017 "Monomorphous Refractory Materials Part 5: Sample Preparation and Pretreatment" for sample preparation, and the bulk density, linear change rate, flexural strength, and compressive strength are tested according to the test method in GB / T4513.6-2017 "Monomorphous Refractory Materials Part 6: Determination of Physical Properties". The qualified product detection index range is: water addition rate is 5.7-6.5wt%; solidification time is 50-120min; bulk density is 2.65-2.85g·cm 3 ; Linear change rate (1100℃ / 3h) is -0.2~0.2%, line change rate (1600℃ / 3h) is 0~0.5%; flexural strength (110℃) is ≥9.5MPa, flexural strength (1100℃ / 3h) is ≥11.5MPa, flexural strength (1600℃ / 3h) is ≥11.5MPa; compressive strength (110℃) is ≥57MPa, compressive strength (1100℃ / 3h) is ≥96MPa, compressive strength (1600℃ / 3h) is ≥114MPa; pouring times is ≥23 times (6-machine 6-stream billet, tundish cover in impact zone); construction performance is good. Test results are shown in Table 1:

[0073] Table 1 Test results of Examples 1 to 6 and Comparative Examples 1 to 4

[0074]

[0075]

[0076] Comparative Example 1 is based on Example 2, but the introduction of aluminum silicate fiber is cancelled, and 15-8mm alumina is added accordingly. As can be seen from Table 1, compared with Example 2, the linear change rate of Comparative Example 1 at 1600℃ / 3h is too large, and the flexural strength and compressive strength are significantly reduced. Only 22 castings are used, and the number of castings is significantly reduced. The test result is unqualified. The test effect of Comparative Example 1 is significantly lower than that of Example 2.

[0077] Comparative Example 2 is based on Example 3, in which the introduction of polyvinyl alcohol is cancelled in the composite binder, and all of it is silica sol. As can be seen from Table 1, compared with Example 3, the water addition rate and solidification time of Comparative Example 2 are increased, and the flexural strength and compressive strength are significantly reduced. Only 23 pouring times are used, and the number of pouring times is significantly reduced. The construction performance is general, and the test results are unqualified. The test effect of Comparative Example 2 is significantly lower than the test effect of Example 3.

[0078] Comparative Example 3 is based on Example 4, but the introduction of ferrosilicon powder is cancelled and 15-8mm alumina is added accordingly. As can be seen from Table 1, compared with Example 4, the flexural strength and compressive strength of Comparative Example 3 at 1600℃ / 3h are significantly reduced. Only 20 pouring times are used, and the number of pouring times is significantly reduced. The test result is unqualified. The test effect of Comparative Example 3 is significantly lower than the test effect of Example 4.

[0079] Comparative Example 4 is based on Example 5, but the introduction of calcium silicate is cancelled and 15-8 mm alumina is added accordingly. As can be seen from Table 1, compared with Example 5, the flexural strength and compressive strength of Comparative Example 4 are significantly reduced. Only 21 pouring times are used, and the number of pouring times is significantly reduced. The test result is unqualified. The test effect of Comparative Example 4 is significantly lower than the test effect of Example 5.

[0080] In summary, the present invention can effectively improve the flexural strength and compressive strength of the tundish cover castable by adding aluminum silicate fiber, ferrosilicon powder and calcium silicate, and the service life is significantly increased. By adding a composite binder combining polyvinyl alcohol and silica sol, the bonding force and plasticity provided by polyvinyl alcohol at low temperature and the strength and stability provided by silica sol at high temperature are utilized, so that the tundish cover castable has both good construction performance and excellent high-temperature performance, and is more suitable for use in harsh high-temperature environments, thereby achieving higher strength, better thermal stability and longer service life of the tundish cover castable.

[0081] The above description is only a preferred embodiment of the present invention and does not limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A long-life tundish cover casting material, Features: The mass percentages of the raw material components in the long-life tundish cover castable are as follows: 5-7% of 15-8mm alumina, 12-14% of 8-5mm alumina, 12-14% of 5-3mm alumina, 22-24% of 3-1mm alumina, 8-10% of 1-0mm alumina, 13-15% of 200-mesh alumina, 1-2% of mullite, 3.5-4.5% of kyanite, and 1% of silicon carbide. .5-2.5%, ferrosilicon powder is 0.2-0.3%, composite binder is 3-4%, calcium silicate is 0.6-0.8%, aluminum silicate fiber is 0.1-0.2%, waste fused bricks are 0.5-0.7%, alumina powder is 2.5-3%, sodium tripolyphosphate is 0.08-0.1%, silica fume is 2.5-3%, organic fiber is 0.02-0.03%, steel fiber is 1%, and high alumina cement is 3-4%.

2. A long-life tundish cover castable according to claim 1, Features: The long-life tundish cover castable contains 6% of 15-8mm alumina, 12.5% ​​of 8-5mm alumina, 13% of 5-3mm alumina, 22.8% of 3-1mm alumina, 9% of 1-0mm alumina, 13.9% of 200-mesh alumina, 1.5% of mullite, 4% of kyanite, 1.9% of silicon carbide, 0.3% of ferrosilicon powder, 3.4% of composite binder, 0.75% of calcium silicate, 0.14% of aluminum silicate fiber, 0.6% of waste fused bricks, 2.8% of alumina powder, 0.09% of sodium tripolyphosphate, 2.8% of silica ash, 0.02% of organic fiber, 1% of steel fiber and 3.5% of high-alumina cement.

3. A long-life tundish cover castable according to claim 1, Features: The Al in the 15-8 mm bauxite 2 O 3 Content ≥80%; Al in 8-5mm alumina 2 O 3 Content ≥80%; Al in 5-3mm alumina 2 O 3 Content ≥85%; Al in 3-1mm alumina 2 O 3 Content ≥85%; Al in 1-0mm alumina 2 O 3 Content ≥87%; Al in 200 mesh alumina 2 O 3 Content ≥87%; mullite is sintered mullite with a mesh size of 200; kyanite particle size is 100 mesh; calcium silicate particle size is 1250 mesh, melting point ≥1500℃; sodium tripolyphosphate is industrial grade; SiO in silica ash 2 Content ≥95%; Al in high alumina cement 2 O 3 Content ≥71%.

4. A long-life tundish cover castable according to claim 1, Features: The mass percentages of the raw material components in the composite binder are as follows: polyvinyl alcohol is 12%, silica sol is 88%, and the effective component content of silica sol is 30%.

5. A long-life tundish cover castable according to claim 1, Features: The mass percentages of the raw material components in the silicon carbide are as follows: 60% of the silicon carbide with a particle size of 80 meshes, and 40% of the silicon carbide with a particle size of 400 meshes.

6. A long-life tundish cover castable according to claim 1, Features: The mass percentages of the raw material components in the alumina fine powder are as follows: 60% of the alumina with a particle size of 1 μm and 40% of the alumina with a particle size of 3 μm.

7. A long-life tundish cover castable according to claim 1, Features: The ferrosilicon powder has a particle size of 200 meshes and its surface is subjected to thermal oxidation treatment.

8. A long-life tundish cover castable according to claim 1, Features: The aluminum silicate fiber has a length of 3-20 mm and a diameter of 1-6 μm.

9. A long-life tundish cover castable according to claim 1, Features: The waste fused bricks are used AZS fused bricks with a particle size of 600 meshes.

10. A long-life tundish cover castable according to claim 1, Features: The castable is suitable for T-type tundish with 5 strands or more.

Citation Information

Patent Citations

  • Magnesia-alumina spinel skinning-resistant non-amorphous refractory material for cement kiln as well as preparation method and application thereof

    CN102391002A

  • Wear-resisting castable refractory

    CN102491770A

  • Ceramic fiber refractory castable and preparation method thereof

    CN109553428A

  • Tundish castable and preparation method thereof

    CN111377715A

  • Tundish cover castable and method for preparing tundish cover by using same

    CN113200753A

Cited By

  • Preparation method of nano high-performance iron runner castable

    CN119409489A

  • A preparation method of nano high-performance iron ditch castable

    CN119409489B

  • Nano ladle magnesia carbon brick and preparation process thereof

    CN120329009A