Regenerated PET composite material and preparation method thereof

Through chain extension, fluorinated graft modification and glass fiber reinforcement of PET materials, combined with thermal filler and twin screw extrusion technology, the problems of insufficient flame retardant performance and mechanical properties of PET materials are solved, and high-performance regenerative PET composite is achieved Material preparation meets high requirements in industrial fields such as automobiles.

CN119060267AInactive Publication Date: 2024-12-03SHANGHAI ZHONGLEI NEW MATERIAL SCI CO LTD

Patent Information

Application Number
CN202411553890.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PET materials have insufficient flame retardant performance, environmental pollution, mechanical performance impact and compatibility problems in the industrial field, and cannot meet the high-demand application needs such as automobiles.

Method used

Using the preparation method of regenerated PET composite materials, through chain extension, fluorinated graft modification, glass fiber reinforcement and thermally conductive filler addition, combined with twin screw extrusion technology, self-flame retardant, enhanced electron transport and heat resistance chemistry were prepared. Composite material with stability and enhances the hydrophobicity and thermal conductivity of the material.

Benefits of technology

It realizes the self-flame retardant of PET materials, enhances electronic transmission and heat resistance chemical stability, and at the same time improves the strength, toughness and leakage resistance of the materials, meeting the high requirements in the automotive and other industrial fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a regenerated PET composite material and a preparation method thereof. The regenerated PET composite material comprises regenerated PET, fluorine-containing acrylate, a chain extender, an initiator, a heat-conducting filler, glass fibers, a fluorine-containing silane coupling agent, a flexibilizer, a lubricant, an antioxidant and a heat stabilizer. The regenerated PET is subjected to chain extension tackifying and fluorination grafting modification, the fluorine-containing silane coupling agent is used for carrying out surface treatment on the glass fibers, and the finally melt-extruded regenerated PET composite material has self-flame retardance, enhanced electron transport and heat-resistant chemical stability, and meanwhile, the strength, toughness and leakage electrical trace resistance of the composite material are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PET regeneration, and in particular to a recycled PET composite material and a preparation method thereof. Background Art

[0002] Polyethylene terephthalate (PET) is a semi-crystalline polyester with a benzene ring, an ester group and a flexible alkane chain structure in the molecular chain. Both ends of the benzene ring are connected to the ester group to form a conjugated structure with extremely rigid chains. The products have excellent wear resistance, heat resistance, and chemical resistance. There are only two flexible fatty chain CH2 structures, which are restricted by the benzene rings. At the same time, the flexible chain length is insufficient, resulting in a slightly slow crystallization rate, requiring high mold temperature. Incomplete crystallization can easily lead to warping problems, but PET materials are temperature-friendly and low-priced. Therefore, modifying them to meet the needs of the industrial field has become an important research direction. At present, polyethylene terephthalate (PET) composite materials, as one of the five major engineering plastics, are widely used in electronics, electrical appliances, communications, and automotive parts.

[0003] PET resin is widely used as a packaging material for drinking water, and is generally used once, which results in great waste of resources and environmental pollution. Therefore, it is of great significance to utilize recycled PET resources. There are many types of PET products used as drinking water bottles, and their components are different, resulting in unstable product performance. At the same time, the molecular chain of recycled products is short and the viscosity is low, so they cannot be directly recycled for industrial use. Chain extension, avoiding the problem of thermal degradation during recycling, and strengthening and toughening have become important improvement directions.

[0004] Processing process of mineral water bottles and other beverage bottles: Classification of mineral water bottles and other beverage bottles: PET water bottles can be divided into carbonated beverage bottles, tea, fruit juice beverage bottles and mineral water beverage bottles. Different categories correspond to different material viscosities, which can be modified separately; Mineral water bottle cleaning: remove non-PET material parts such as bottle caps and labels, clean and dry; Crushing: Put the mineral water bottles that have been initially cleaned into the crusher, crush them, and then clean and dry them again for use.

[0005] At present, for new energy vehicles, three-electric thermal management system parts, the requirements for material flame retardancy and electrical properties are increased. The oxygen index of PET material is about 20, which is a flammable material, so it needs to be flame-retardant modified. Commonly used flame retardants are halogen flame retardants, such as bromine-antimony synergistic flame retardants, but they cannot meet the growing environmental protection requirements. The second type is organic hypophosphite flame retardants, which have excellent flame retardancy and electrical properties, but because the decomposition products are acidic, PET is easily degraded during processing. The third type is inorganic aluminum hypophosphite flame retardants. The addition of inorganic fillers affects the processing type and the overall mechanical properties of the product. The addition of flame retardants improves the flame retardant properties, but the content is often very high, which affects the overall mechanical properties. At the same time, its compatibility problems will also lead to the precipitation of flame retardants, decreased flame retardant ability, and induced material degradation during subsequent use. Therefore, it cannot meet the demand for flame retardant properties of materials in industrial fields such as automobiles.

[0006] For example, the patent document with publication number CN109749376A discloses a technical solution, which actually uses bromine antimony flame retardant compounded with melamine polyphosphate and aluminum hypophosphite. The addition amount exceeds 30% to achieve flame retardancy, and the CTI reaches 340V. The addition of a large amount of flame retardant has a great influence on the overall mechanical properties of the material. At the same time, the bromine antimony flame retardant will cause a certain degree of pollution to the environment.

[0007] Patent document with publication number CN112300543A discloses a technical solution, which actually uses PBT and PET materials to compound and add flame retardants to achieve CTI400V. A small amount of flame retardant cannot achieve high performance flame retardancy.

[0008] The patent document with publication number CN112300543A discloses a technical solution, which modifies PET material by adding methyl ethyl zinc hypophosphite (Zn~MEP) and nitrogen-based melamine cyanurate (MCA) flame retardant, and the flame retardant grade can reach UL94 V~0. However, the system is a fiber-free flame retardant system, and does not solve the compatibility problem between halogen-free flame retardant and glass fiber. In addition, the physical and mechanical properties and heat resistance of the fiber-free flame retardant system are insufficient, and the CTI index is not significantly improved, which greatly limits the application of the material. Regarding recycled PET materials, a patent document with publication number CN115895205A discloses a technical solution, which recycles PET materials used in the ocean, adds PBT materials for compound modification, and adds chain extenders and composite flame retardants to achieve rigidity and toughness improvement modifications, and the impact performance is greatly improved. However, there is no glass fiber reinforcement, the overall strength is insufficient, the heat resistance is insufficient, and it does not have sufficient flame retardancy, and cannot meet the requirements of larger industrial fields such as automobiles.

[0009] The patent document with publication number CN114805766A discloses a technical solution, which modifies waste PET with PBT compound, first depolymerizes the recycled material into BHET and BHBT monomers, and then carries out ester exchange and polycondensation. The whole process has high energy consumption, and polycondensation after depolymerization into monomers increases the difficulty of reaction control, and it is difficult to ensure the treatment effect of side reactions. The advantages of the original finished product are lost, and the obtained product cannot be directly used for industrial use, and further modification is required. The modification scheme has limitations. Summary of the invention

[0010] In view of the above-mentioned deficiencies of the current recycled PET materials, the present invention provides a recycled PET composite material and a preparation method thereof, which can realize the self-flaming retardancy of the material, enhance the electron transmission and heat-resistant chemical stability, and at the same time improve the hydrophobicity of the material, and enhance the strength, toughness and electrical leakage and tracking resistance of the composite material.

[0011] To achieve the above object, the embodiments of the present invention adopt the following technical solutions: A recycled PET composite material is prepared from the following raw materials in parts by weight: Recycled PET 50~80 parts; 10-30 parts of fluorinated acrylate; Chain extender 0.1~1 part; Initiator 0.1~1 part; 3~15 parts of thermal conductive filler; Glass fiber 10~40 parts; 2~8 parts of fluorinated silane coupling agent; Toughening agent 0.2~5 parts; Lubricant 0.1~2 parts; Antioxidant 0.2~1 part; Heat stabilizer 0.2~1 part.

[0012] Preferably, the chain extender is one or more of glycidyl ester chain extender, maleic anhydride, pyromellitic dianhydride PMDA, and 1,6-hexamethylene diisocyanate (HMDI).

[0013] Preferably, the initiator is one or more of ethylene glycol, benzyl alcohol, benzyl alcohol, and hyperbranched polyether.

[0014] Preferably, the thermally conductive filler is one or more of aluminum nitride, flaky micron-sized hexagonal boron nitride, aluminum oxide, zinc oxide and magnesium oxide.

[0015] Preferably, the rPET comes from sorted recycled plastic bottles.

[0016] Preferably, the fluorine-containing acrylate is pentafluoropropyl acrylate.

[0017] Preferably, the fluorine-containing silane coupling agent is tridecafluorooctyltriethoxysilane (FAS).

[0018] Preferably, the antioxidant is one or more of antioxidant 1076 and TAS~A.

[0019] On the other hand, the present invention provides a method for preparing a recycled PET composite material, which is used to prepare the above-mentioned recycled PET composite material, and comprises the following steps: Chain extension and viscosity enhancement: Use acid hydrolysis or alcoholysis to pretreat recycled PET, and use chain extenders for chain extension modification; Fluorination grafting modification: adding fluorinated acrylate to recycled PET and using an initiator to carry out ester exchange reaction or hydrolysis ester exchange reaction to achieve graft copolymerization of fluorinated chain segments with PET; Glass fiber reinforcement: Use fluorinated silane coupling agent to treat the glass fiber surface to obtain treated glass fiber; Melt extrusion: The recycled PET modified by chain extension, viscosity enhancement and fluorination grafting, thermal conductive filler, treated glass fiber, toughening agent, lubricant, antioxidant and thermal stabilizer are mixed, and the mixture is melt-extruded and granulated to obtain a recycled PET composite material.

[0020] Preferably, the melt extrusion process is carried out in a twin-screw extruder, the processing temperature of the twin-screw extruder is 190-290° C., and the screw speed is 200-400 rpm.

[0021] Preferably, the mixture is preheated and dried before being melt extruded.

[0022] Advantages of the implementation of the present invention: The present invention increases the reactivity of recycled PET by pre-treating it, significantly increases the length of the chain segment and the intrinsic viscosity by using a chain extender, and introduces fluorinated grafting modification to achieve self-flaming retardancy, enhance electron transport and heat-resistant chemical stability, while improving the hydrophobicity of the material. In addition, a fluorinated silane coupling agent is used to treat the glass fiber to improve its compatibility with the PET matrix, and to enhance the strength, toughness and resistance to electrical leakage traces of the composite material. Hexagonal boron nitride is added as a thermally conductive filler to effectively improve thermal conductivity. Finally, efficient melt extrusion is achieved through a twin-screw extruder to prepare a recycled PET composite material with excellent performance, providing an innovative solution for the high-value utilization of recycled PET. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The preparation method of embodiments 1 to 9 comprises the following steps: Chain extension and viscosity enhancement: Use acid hydrolysis or alcoholysis to pretreat recycled PET, and use chain extenders for chain extension modification; Among them, the recycled PET material contains certain active hydroxyl end groups and carboxyl end groups due to the use and existence of a certain degree of thermal degradation. The end group concentration of the relatively high viscosity PET recycled material is insufficient, so it will be pre-depolymerized by acid hydrolysis to control the reaction process and the amount of addition so that it contains higher hydroxyl end groups and carboxyl end groups. For example, diols are used for alcoholysis. There are many types of diols, such as ethylene glycol alcoholysis. Using diol alcoholysis can produce unsaturated PET containing active hydroxyl and carboxyl groups, which can be used for subsequent chain extension, capacity expansion and reactive grafting of fluorinated chain segments.

[0025] A variety of effective chain extenders can be used to extend the chain of PET, including epoxy chain extenders, such as SMC, glycidyl ester chain extenders (711, TDE85, preferred in this work), ECY (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), diepoxy functional groups or polyepoxy functional groups (TGGDM) to extend the chain of PET, which can greatly increase the chain length and improve the molecular chain and intrinsic viscosity.

[0026] Fluorination grafting modification: adding fluorinated acrylate to recycled PET and using an initiator to carry out ester exchange reaction or hydrolysis ester exchange reaction to achieve graft copolymerization of fluorinated chain segments with PET; The recycled PET is modified by fluorination grafting to achieve self-flame retardancy. At the same time, the fluorinated structure can capture electrons, enhance electron transmission, reduce failure behaviors such as flashover caused by charge accumulation, and enhance the CTI of the material.

[0027] The fluorine element has a large electronegativity, and CF can achieve high polarization. After grafting the fluorine-containing segments, under high voltage, the CF structure can capture a large number of electrons to achieve a good electron shielding layer, preventing the continuous internal accumulation of space charges and avoiding local flashover and breakdown caused by charge accumulation; the CF bond energy is large, 485KJ / mol, which is greater than the CH bond energy of 410KJ / mol and the CC bond energy of 368KJ / mol. Adjacent F atoms repel each other, so that they are not in the same plane, and can form a tight coating on the C atoms, thereby achieving internal protection and enhancing the heat resistance and chemical stability of the matrix; and the surface energy of fluorine atoms is very low, and the symmetrical arrangement of the structure greatly improves the hydrophobicity of the material and the ability of the material surface to resist dirt.

[0028] The present invention uses two approaches to achieve fluorine-containing graft-modified PET materials. One is to add fluorine-containing acrylates, such as pentafluoropropyl acrylate (preferred in the present invention), octafluoropentyl methacrylate, hexafluorobutyl methacrylate, etc., and use polyethers, alcohols, such as hyperbranched polyethers (having polydispersity and multiple hydroxyl initiation points on the surface to achieve block polymerization), benzyl alcohol, benzyl alcohol and other ester exchange initiators to achieve alcoholysis ester exchange reaction, and achieve graft copolymerization reaction of fluorine-containing hyperbranched blocks with recycled PET materials containing terminal hydroxyl groups and terminal carboxyl groups (direct ester exchange and hydrolysis ester exchange are also possible).

[0029] Glass fiber reinforcement: Use fluorinated silane coupling agent to treat the glass fiber surface to obtain treated glass fiber. This step improves the compatibility of glass fiber and PET matrix. Melt extrusion: The recycled PET modified by chain extension, viscosity enhancement and fluorination grafting, thermal conductive filler, treated glass fiber, toughening agent, lubricant, antioxidant and thermal stabilizer are mixed, and the mixture is melt-extruded and granulated to obtain a recycled PET composite material.

[0030] Among them, fluorinated siloxane coupling agents, such as tridecafluorooctyl triethoxysilane (FAS), can be used to treat glass fibers to enhance the bonding between glass fibers and the matrix, enhance interfacial compatibility, and make the composite material have better strength and toughness. Use fluorinated silane coupling agents to treat glass fibers, so that the surface of the glass fibers contains fluorinated segments, which enhances the bonding with fluorinated modified PET materials. At the same time, the introduction of recovery rent makes the entire matrix, glass fibers and PET tightly covered under the fluorinated layer, which can enhance the composite material's resistance to electrical tracking. The oxygen index of the composite material was tested and it was found that the oxygen index of the fluorinated composite material could be increased to 36~45%, giving priority to achieving self-flame retardant properties.

[0031] Among them, hexagonal boron nitride has a high thermal conductivity of 33W / m·K, and its thermal conductivity is even better under high temperature conditions. When added to the matrix, it greatly improves the thermal conductivity of the material, reduces heat accumulation, and avoids high-temperature flashover-induced large-scale carbonization of the tree surface and causes surface insulation failure. The selection of flaky hexagonal boron nitride can better form a uniform thermal conductive sheet network structure, and the thermal conductivity is increased to 2.5~4W / m·K.

[0032] The melt extrusion process is carried out in a twin-screw extruder, the processing temperature of the twin-screw extruder is 190~290℃, and the screw speed is 200~400rpm.

[0033] The raw material ratio is shown in Table 1.

[0034]

[0035] The material properties are shown in Table 2.

[0036]

[0037] The comparative example is shown in Table 3, and the specific implementation steps are the same as those of Examples 1 to 7.

[0038]

[0039]

[0040] Through the analysis of the above comparative example 2 and examples 4-5, it can be concluded that the optimal dosage of the chain extender is 0.8, and the addition of the chain extender can effectively enhance the tensile strength; through the analysis of the above comparative example 3 and examples 6-7, it can be concluded that the thermal conductive filler has a greater impact on CTI, and the CTI can be significantly increased by adding the thermal conductive filler; through the analysis of the above comparative examples 4-5 and examples 8-9, it can be concluded that the benzyl alcohol used in comparative example 4 can also realize the graft copolymerization reaction of the fluorinated hyperbranched block and the recycled PET material containing terminal hydroxyl groups and terminal carboxyl groups, and the effect is better when ethylene glycol is used as the initiator, wherein the optimal dosage of ethylene glycol is 0.5; through the analysis of comparative example 6 and examples 1-9, the content of glass fiber affects the strength of the PET composite material, and too little glass fiber content will increase the fracture of the PET composite material; through the analysis of examples 1-3, it can be concluded that when the fluorinated acrylate is too little, the flame retardancy and CTI are insufficient, and when the fluorinated acrylate is too much, the improvement effect is not obvious, and the preferred dosage is 5.

[0041] Advantages of the implementation of the present invention: The present invention increases the reactivity of recycled PET by pre-treating it, significantly increases the length of the chain segment and the intrinsic viscosity by using a chain extender, and introduces fluorinated grafting modification to achieve self-flaming retardancy, enhance electron transport and heat-resistant chemical stability, while improving the hydrophobicity of the material. In addition, a fluorinated silane coupling agent is used to treat the glass fiber to improve its compatibility with the PET matrix, and to enhance the strength, toughness and resistance to electrical leakage traces of the composite material. Hexagonal boron nitride is added as a thermally conductive filler to effectively improve thermal conductivity. Finally, efficient melt extrusion is achieved through a twin-screw extruder to prepare a recycled PET composite material with excellent performance, providing an innovative solution for the high-value utilization of recycled PET.

[0042] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A recycled PET composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Recycled PET 50~80 parts; 10-30 parts of fluorinated acrylate; Chain extender 0.1~1 part; Initiator 0.1~1 part; 3~15 parts of thermal conductive filler; Glass fiber 10~40 parts; 2~8 parts of fluorinated silane coupling agent; Toughening agent 0.2~5 parts; Lubricant 0.1~2 parts; Antioxidant 0.2~1 part; Heat stabilizer 0.2~1 part.

2. The recycled PET composite material according to claim 1, characterized in that: The chain extender is one or more of glycidyl ester chain extender, maleic anhydride, pyromellitic dianhydride PMDA, and 1,6-hexanediisocyanate.

3. The recycled PET composite material according to claim 1, characterized in that: The initiator is one or more of ethylene glycol, benzyl alcohol, benzyl alcohol and hyperbranched polyether.

4. The recycled PET composite material according to claim 1, characterized in that: The thermal conductive filler is one or more of aluminum nitride, flaky micron-sized hexagonal boron nitride, aluminum oxide, zinc oxide and magnesium oxide.

5. The recycled PET composite material according to claim 1, characterized in that: The recycled PET comes from sorted recycled plastic bottles.

6. The recycled PET composite material according to claim 1, characterized in that: The fluorine-containing acrylate is pentafluoropropyl acrylate.

7. The recycled PET composite material according to claim 1, characterized in that: The fluorine-containing silane coupling agent is tridecafluorooctyltriethoxysilane.

8. The recycled PET composite material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1076 and TAS~A.

9. A method for preparing a recycled PET composite material, for preparing the recycled PET composite material according to any one of claims 1 to 8, characterized in that: The steps include: Chain extension and viscosity enhancement: Use acid hydrolysis or alcoholysis to pretreat recycled PET, and use chain extenders for chain extension modification; Fluorination grafting modification: adding fluorinated acrylate to recycled PET and using an initiator to achieve graft copolymerization of fluorinated chain segments with PET; Glass fiber reinforcement: Use fluorinated silane coupling agent to treat the glass fiber surface to obtain treated glass fiber; Melt extrusion: The recycled PET modified by chain extension, viscosity enhancement and fluorination grafting, thermal conductive filler, treated glass fiber, toughening agent, lubricant, antioxidant and thermal stabilizer are mixed, and the mixture is melt-extruded and granulated to obtain a recycled PET composite material.

10. The preparation method according to claim 9, characterized in that: The melt extrusion process is carried out in a twin-screw extruder, the processing temperature of the twin-screw extruder is 190-290° C., and the screw speed is 200-400 rpm.

Citation Information

Patent Citations

  • Method for tackifying recycled polyester bottle flake by using chain extender and application thereof

    CN109749070A

  • Method for preparing unsaturated polyester resin by using waste polyester textile fabrics as raw material

    CN110156932A

  • Temperature-resistant and yellowing-resistant PET master batch and preparation method thereof

    CN115627046A

  • Composite material for bearing retainer and preparation method of composite material

    CN117024952A

  • Copolyetherester and method for producing the same

    JP2002012658A

Cited By

  • Impact-resistant high-thermal-conductivity regenerated PET composite material and preparation method thereof

    CN119286041A

  • Regenerated PET composite material and preparation method thereof

    CN119875327A