High-elastic polyimide aerogel and green preparation method thereof
By adding active capping agent to the synthesis of polyimide aerogel for crosslinking, the problem of poor mechanical properties is solved, and the polyimide aerogel with high elasticity and mechanical properties is formed, which broadens its application fields .
Patent Information
- Application Number
- CN202411263678.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-03
AI Technical Summary
The problems of poor mechanical properties of polyimide aerogels and the use of large amounts of organic solvents and expensive crosslinking agents during preparation limit their application areas.
The molecular chains are crosslinked by adding active capping agents during polyimide synthesis to enhance the three-dimensional network structure and mechanical properties of the aerogel, using diamine monomers 3,5-diaminobenzoic acid and diamine monomers The anhydride monomer 4,4'-oxybisphthalic anhydride is used to promote the cross-linking reaction through acetic anhydride and triethylamine to form a polyimide aerogel with high elasticity and mechanical properties.
It significantly improves the elasticity and mechanical properties of polyimide aerogel, reduces density, and relieves the concentration of compressive stress through cross-linking nodes, improving the mechanical strength and application advantages of aerogel.
Smart Images

Figure CN119060401A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material preparation, and particularly relates to a high-elastic polyimide aerogel and a green preparation method thereof. Background Art
[0002] Polyimide aerogels not only maintain the excellent comprehensive properties of polyimide itself, but also have the characteristics of aerogels such as low refractive index, low thermal conductivity, low dielectric constant, low density, and high specific surface area. However, they have problems such as large shrinkage, poor mechanical properties, and the use of a large amount of organic solvents and expensive chemical cross-linking agents during the preparation process. Therefore, how to improve the mechanical properties and environmental friendliness of polyimide aerogels is the key to further broadening the application field of polyimide aerogel materials.
[0003] The preparation of cross-linkable polyimide has been proven to be a successful method to improve its mechanical properties, because the cross-linked polyimide material has more outstanding comprehensive properties. However, the cross-linking agents used in existing cross-linkable polyimide include trimesoyl chloride, 1,3,5-tris(4-aminophenoxy)benzene, TAPP, etc., which have relatively complex structures and high prices. Summary of the invention
[0004] In order to solve the problem of poor mechanical strength of polyimide aerogel pointed out in the background technology part, the present invention adds an active end-capping agent during the synthesis of polyimide through molecular design to cross-link the polyimide molecular chains, thereby enhancing the three-dimensional network structure of the aerogel prepared thereby, improving the elasticity of the aerogel, solving the problem of limited application in certain fields due to poor elasticity, and at the same time improving the mechanical strength of the polyimide aerogel.
[0005] The novel end-capped cross-linked polyimide aerogel provided by the present invention has good elasticity and good mechanical properties. The highly elastic polyimide aerogel has the following structure, taking the diamine monomer as 3,5-diaminobenzoic acid and the dianhydride monomer as 4,4'-oxydiphthalic anhydride as an example:
[0006]
[0007] Among them, 10 <n<2000。
[0008] The novel highly elastic polyimide aerogel provided by the present invention is prepared according to the following steps:
[0009] (1) Preparation of polyimide water aerogel
[0010] Add 45 ml of dehydrated DMAc to a three-necked flask, and add 3,5-diaminobenzoic acid (DABA), replace with nitrogen 3 times to ensure that the air in the device is removed, and stir until it is completely dissolved. Add dianhydride monomer 4,4'-oxydiphthalic anhydride (ODPA) in small amounts and multiple times (5 times) to ensure that the ends of the molecular chain are amino-terminated, observe the viscosity, and after reacting for 8 hours, add the end-capping agent maleic anhydride (MA), react for 1 hour, add acetic anhydride (AA) and triethylamine (TEA) and continue to react for 3 hours to obtain a gel.
[0011] The diamine monomer may also be 6,6′-bisamino-3,3′-methylenedibenzoic acid (MBAA).
[0012] The dianhydride monomer may also be one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3',4-biphenyltetracarboxylic dianhydride (α-BPDA), and (4-phthalic anhydride) formyloxy-4-phthalate (8Cl).
[0013] The molar ratio of the dianhydride monomer, the diamine monomer, maleic anhydride, acetic anhydride and triethylamine is 11:10:10:20:20.
[0014] Among them, the role of acetic anhydride is to carry out imidization, and triethylamine mainly plays the role of a catalyst to promote the formation of the polymer and adjust the molecular weight, molecular weight distribution and properties of the polyamide.
[0015] (2) The above product was poured into a container for gel aging for 24 hours, and the aged gel was placed in a mixed solution of methanol and DMAc for solvent replacement. The solvent was replaced every 6 hours, and a hydrogel was obtained after 5 replacements.
[0016] The solvent used in the replacement is a mixed solvent of methanol and DMAc, and the volume-to-mass ratio thereof is 4:1-1:4. The volume ratio of the mixed solution to the gel is 100:1.
[0017] (3) Drying the prepared hydrogel in a vacuum oven at a temperature of 60° C. ≤ 80° C. and a vacuum degree of ≤ 133 Pa for 12 h to obtain a polyimide aerogel.
[0018] Beneficial Effects
[0019] The highly elastic polyimide aerogel prepared by the present invention has a novel structure and good elasticity and mechanical properties, which makes this type of polyimide aerogel have great advantages in mechanical applications. In addition, the surface of the prepared aerogel contains polar groups, which can generate interactive forces on polar molecules and can be applied in extrusion adsorption and other aspects, which is different from traditional aerogels. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the cycle curve of the polyimide aerogel (PI Aerogel) synthesized in Example 1 when it is compressed to 80%.
[0021] Figure 2 These are stress-strain curves of the polyimide aerogel (PI Aerogel) synthesized in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0022] In order to explain the present invention more clearly, the present invention is further described below in conjunction with embodiments. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0023] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods. The experimental materials, reagents, etc. used in the following experimental examples can be obtained through commercial channels or known experimental methods.
[0024] Example 1
[0025] This embodiment provides a polyimide aerogel having the following structure, and the polyimide aerogel is named ODPA-DABA-MA.
[0026]
[0027] n is a repeating structural unit, ranging from 10 to 2000;
[0028] The preparation method of polyimide aerogel ODPA-DABA-MA is as follows:
[0029] (1) Water removal and purification of N-dimethylacetamide (DMAc):
[0030] Put 55ml of DMAc into a 100ml single-necked flask, add a magnetic bar and 0.5g of CaH2, seal it with a balloon, and stir it magnetically at room temperature for 24 hours to fully react. After the reaction is complete, perform vacuum distillation, separate the front and back fractions, and collect and seal the rest. Yield: 85%.
[0031] (2) Preparation of polyimide water aerogel
[0032] Add 45 ml of dehydrated DMAc to a three-necked flask equipped with a mechanical stirring device, and add 3,5-diaminobenzoic acid DABA (1.5215 g, 11 mmol), replace with nitrogen 3 times to ensure that the air in the device is removed, and stir until it is completely dissolved. Add the dianhydride monomer 4,4'-oxydiphthalic anhydride (ODPA) (3.10215 g, 10 mmol) in small amounts and multiple times (5 times) to ensure that the end of the molecular chain is amino-terminated, observe the viscosity until it hangs on the wall without dripping, react at room temperature for 8 hours, add the end-capping agent maleic anhydride (MA) (9.806 g, 10 mmol), add acetic anhydride AA (2.0418 g, 20 mmol) and triethylamine TEA (2.02386 g, 20 mmol) and continue to react at room temperature for 3 hours to obtain a gel.
[0033] (3) The gel was poured into a container for aging at room temperature for 24 hours, and the aged gel was placed in a mixed solution of methanol and DMAc for solvent replacement. The solvent was replaced every 6 hours, and the hydrogel was obtained after 5 replacements. In the solvents used in the 5 replacements, the volume mass ratio of methanol:DMAc was 4:1, and the volume ratio of the mixed solution to the gel was 100:1.
[0034] (4) Drying the prepared hydrogel in a vacuum oven at a temperature of 60° C. ≤ 80° C. and a vacuum degree of ≤ 133 Pa for 12 h to obtain a polyimide aerogel.
[0035] Infrared data: FTIR (KBr, ν, cm -1 ): 3457, 1717, 1602, 1476, 1370, 1283, 1093, 834, 745.
[0036] Example 2
[0037] The difference between this embodiment and embodiment 1 is that the dianhydride monomer used is 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), and the other treatment methods are the same as those in embodiment 1.
[0038] The compressive strength of the PI aerogel after compression by 80% is 10.79 MPa.
[0039] Infrared data: FTIR (KBr, ν, cm -1 ): 3459, 1718, 1602, 1477, 1367, 1275, 1093, 834, 745.
[0040] The structure is as follows:
[0041]
[0042] Example 3
[0043] The difference between this embodiment and embodiment 1 is that the dianhydride monomer used is 2,3,3',4-biphenyltetracarboxylic dianhydride (α-BPDA), and the other processing methods are the same as those in embodiment 1.
[0044] The compressive strength of the PI aerogel after compression by 80% is 8.88 MPa.
[0045] Infrared data: FTIR (KBr, ν, cm -1 ): 3489, 1718, 1608, 1477, 1367, 1276, 1093, 834, 745.
[0046] The structure is as follows:
[0047]
[0048] Example 4
[0049] The difference between this comparative example and Example 1 is that the diamine monomer used in the synthesis of the polyamic acid PAA precursor in step (2) is 6,6'-bisamino-3,3'-methylenedibenzoic acid (MBAA), and the other treatment methods are the same as those in Example 1.
[0050] The structure is as follows:
[0051]
[0052] Example 5
[0053] The difference between this comparative example and Example 1 is that during the solvent replacement, the volume mass ratio of methanol:DMAc is 1:1, and the other treatment methods are consistent with those in Example 1.
[0054] Example 6
[0055] The difference between this comparative example and Example 1 is that during the solvent replacement, the volume mass ratio of methanol:DMAc is 2:3, and the other treatment methods are consistent with those in Example 1.
[0056] Example 7
[0057] The difference between this comparative example and Example 1 is that during the solvent replacement, the volume mass ratio of methanol:DMAc is 1:4, and the other treatment methods are consistent with those in Example 1.
[0058] Example 8
[0059] The difference between this comparative example and Example 1 is that during the solvent replacement, the volume mass ratio of methanol:DMAc is 3:2, and the other treatment methods are consistent with those in Example 1.
[0060] Comparative Example 1
[0061] The difference between this comparative example and Example 1 is that no end-capping cross-linking agent is added in step (2), and the other treatment methods are consistent with those in Example 1.
[0062] The compressive strength of the PI aerogel when compressed by 80% is 4.87 MPa.
[0063] Infrared data: FTIR (KBr, ν, cm -1 ): 3427, 1717, 1602, 1475, 1357, 1270, 1093, 834, 745.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 1 is that the dianhydride monomer used in the synthesis of the polyamic acid PAA precursor in step (2) is pyromellitic anhydride (PMDA), and the other processing methods are consistent with those in Example 1.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 1 is that the end-capping cross-linking agent used in the synthesis of the PAA precursor in step (2) is 4-phenylethynylphthalic anhydride (PEPA), and the other treatment methods are consistent with those in Example 1.
[0068] The following performance tests were performed on the novel water-soluble end-capped cross-linked polyimide aerogels prepared in Examples 1-8 and Comparative Examples 1-3. The test results are shown in Table 1:
[0069] Mechanical properties test: The polyimide aerogel was tested by a WDT-10KN electronic universal testing machine.
[0070] The density of aerogel is the volume density. The sample used is cylindrical, and its height and bottom diameter are measured. The mass of aerogel is then weighed by an electronic analytical balance.
[0071] From the results in Table 1, it can be seen that the mechanical properties of the polyimide aerogel prepared in Comparative Example 1 are lower than those in Example 1. This is because the addition of the cross-linking agent links the polyimide molecular chains, and a three-dimensional network structure is formed inside the aerogel during thermal imidization. The cross-linked nodes can alleviate the stress concentration phenomenon during compression, thereby improving the mechanical properties of the aerogel.
[0072] Table 1
[0073] sample <![CDATA[Density g / cm 3 > Mass Compression strength MPa Example 1 0.0936 0.4202 20.05 Example 2 0.0636 0.4071 10.79 Example 3 0.0638 0.4098 8.88 Example 4 0.0903 0.4049 18.23 Example 5 0.1001 0.4221 17.36 Example 6 0.1019 0.4302 16.45 Example 7 0.1050 0.4317 15.72 Example 8 0.0942 0.4287 18.02 Comparative Example 1 0.0979 0.5981 4.87 Comparative Example 2 0.0976 0.4882 5.49 Comparative Example 3 0.0929 0.6839 6.21
[0074] From the results in Table 1, it can be seen that the prepared polyimide composite aerogel has a lower density. After adding the end-capping cross-linking agent, the compressive strength of the aerogel is significantly improved.
[0075] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A highly elastic polyimide aerogel, It is characterized in that The aerogel is prepared by preliminarily reacting a dianhydride monomer and a diamine monomer in a solvent, adding a blocking crosslinking agent to obtain a blocking precursor, and then adding acetic anhydride and triethylamine to the precursor for catalytic reaction to obtain a gel, and after aging, the gel is subjected to solvent replacement to obtain a polyimide hydrogel; and then vacuum drying is performed to obtain a polyimide aerogel; Among them, the structures of dianhydride monomer, dianhydride monomer, and end-capping crosslinking agent are as follows:
2. A method for preparing the highly elastic polyimide aerogel according to claim 1, It is characterized in that The preparation method steps are as follows: (1) In a purified NN dimethylacetamide solvent, a diamine monomer is reacted with a dianhydride monomer and maleic anhydride, and then acetic anhydride and triethylamine are added to catalyze the reaction to obtain a gel; (2) pouring the gel obtained in step (1) into a container and aging at room temperature for 24 hours to form a polyimide hydrogel; performing solvent replacement on the prepared hydrogel 5 times; (3) placing the hydrogel after solvent replacement in step (2) into a vacuum oven for drying to obtain a polyimide aerogel.
3. The method for preparing the highly elastic polyimide aerogel according to claim 2, It is characterized in that In step (1), the molar ratio of the dianhydride monomer, the diamine monomer, maleic anhydride, acetic anhydride and triethylamine is 11:10:10:20:
20.
4. The method for preparing the highly elastic polyimide aerogel according to claim 2, It is characterized in that In step (2), in the five solvent replacements, the volume mass ratio of methanol to DMAc was 4:1-1:4, each solvent replacement was performed at an interval of 6 hours, and the volume ratio of the mixed solution to the gel was 100:
1.
5. The method for preparing the highly elastic polyimide aerogel according to claim 2, It is characterized in that In step (3), the vacuum drying conditions are: 60°C≤temperature≤80°C, vacuum degree≤133Pa, and vacuum drying for 12h.
Citation Information
Cited By
Preparation method of composite multifunctional PI aerogel
CN119978528A