Fireproof coating for power battery pack of new energy automobile and preparation method of fireproof coating
By using solvent-free epoxy resin and liquid flame retardant combinations, the problems of difficult mixing, precipitation and high energy consumption of fire-retardant coatings for power battery packs of new energy vehicles are solved, and a coating with homogeneous, non-segmentation and excellent fire-retardation performance is achieved. Prepared, suitable for fire protection of battery packs.
Patent Information
- Application Number
- CN202411331882.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The fire-retardant coatings in existing new energy vehicle power battery packs have problems such as difficulty in mixing, easy precipitation, high energy consumption for preparation, and low production efficiency.
Use solvent-free epoxy resin to replace the aqueous epoxy resin emulsion, combine with liquid flame retardant and solubilizer, and synergistically integrate with the epoxy resin by preferential solid flame retardant additives and inorganic fillers to form homogeneous, non-settling and fire-resistant Excellent fire-retardant coating.
It has achieved homogeneous, no settlement and low energy consumption fire-resistant coating preparation, with excellent fire insulation performance, high temperature resistance, adhesive performance and adhesion, and is suitable for the fire protection of battery packs of new energy vehicles.
Smart Images

Figure BDA0005057193010000021 
Figure BDA0005057193010000022 
Figure BDA0005057193010000051
Abstract
Description
Technical Field
[0001] The present invention relates to a fire retardant coating for a new energy vehicle power battery pack and a preparation method thereof, and is applied in the field of fire retardant coating production for new energy vehicle power battery packs. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] The safety of battery modules of new energy vehicles (pure electric, plug-in hybrid, etc.) is crucial to the safety of new energy vehicles. When a battery module fails, in order to maximize the protection of the driver and passengers in the car, the battery pack needs to be treated with fireproof and heat-insulated treatment to reserve sufficient escape time for the people in the car. At present, the fireproof materials of various new energy vehicle battery packs are mainly laid with fireproof felt materials, such as mica boards, ultra-fine glass wool, high-silica wool felt, etc. When the battery has thermal runaway, relying on fireproof felt materials can effectively isolate the heat diffusion and control the direction of the fire, effectively delaying the thermal diffusion time of the battery, thereby improving the fire safety of the battery pack. However, the solution of adding fireproof felt also has problems such as increased mass, poor heat dissipation performance, and some limitations in the design and construction process. In order to solve these problems, fireproof coatings for new energy vehicle power battery packs came into being.
[0004] Chinese invention patent CN 111100526 A discloses an aerogel thermal insulation coating for aluminum alloy battery packs, which achieves fireproof performance by adding tributyl phosphate, ammonium polyphosphate, aluminum hydroxide, expanded graphite and other flame retardants to water-based epoxy resin emulsion. However, adding aluminum hydroxide, expanded graphite and other flame retardants to the emulsion cannot be well dispersed in the emulsion. As the placement time increases, the flame retardant is prone to precipitation, which in turn affects the performance of the fire retardant coating.
[0005] Chinese patent CN 115260817 A also discloses a fire retardant coating for new energy vehicle battery packs. This patent has developed a new dispersant to address the problem of flame retardant precipitation. The dispersant is specially developed to improve the dispersibility of zinc borate in emulsions. However, to prepare this dispersant, the reactor needs to be heated to a higher temperature (120-150°C) and maintained for a long time (4-8h), which will generate a lot of energy consumption and greatly reduce production efficiency.
[0006] Therefore, it has become an urgent task to provide a fire retardant coating for new energy vehicle power battery packs, which can be prepared by low energy consumption means, is homogeneous, has no sedimentation and has excellent fire retardant performance, and a preparation method thereof. Summary of the invention
[0007] In order to overcome the shortcomings of existing fire-retardant coatings for new energy vehicle power battery packs, such as difficulty in mixing, easy precipitation, high energy consumption for preparation, and low production efficiency, the present invention provides a fire-retardant coating for new energy vehicle power battery packs and a preparation method thereof. Solvent-free epoxy resin is used to replace the water-based epoxy resin emulsion commonly used in existing fire-retardant coatings, and liquid flame retardants and solubilizers are added. Solid flame retardant additives, inorganic fillers and epoxy resins are preferably selected for synergistic enhancement, so that the coating has the advantages of homogeneity, no sedimentation and excellent fire resistance.
[0008] The technical solution of the present invention is as follows:
[0009] A fire retardant coating for a new energy vehicle power battery pack, comprising the following component A and component B:
[0010] Wherein, the A component is mainly prepared from the following components in the following weight ratios:
[0011]
[0012] The B component is mainly prepared from the following components in the following weight ratios:
[0013]
[0014] The solid flame retardant additive in component A is ammonium polyphosphate, and the solid flame retardant additive in component B is a combination of ammonium polyphosphate and melamine in any proportion.
[0015] The fire retardant coating for the power battery pack of new energy vehicles in this application uses solvent-free epoxy resin to replace the water-based epoxy resin emulsion commonly used in existing fire retardant coatings, and is combined with liquid flame retardants and solubilizers, and through the preferred solid flame retardant additives, inorganic fillers and epoxy resins for synergistic synergy, it has the advantages of homogeneity, no sedimentation and excellent fire retardant performance. The specific mechanism is as follows: This case solves the disadvantage of poor dispersibility of flame retardant fillers in the system by using solvent-free epoxy resin to replace the water-based epoxy resin emulsion commonly used in the existing fire retardant coating system; the added liquid flame retardant can, on the one hand, synergistically enhance the effect and achieve good fireproof and heat insulation performance, and on the other hand, it can be used as a solvent to improve the problem of poor miscibility of solids and liquids in the system, and achieve homogeneous coating without precipitation. The fire retardant coating in this case does not need to add the additional special dispersant synthesized by high energy consumption as described in patent CN 115260817 A, and can solve the problem of flame retardant precipitation. In addition, this case uses a solid flame retardant additive (a combination of melamine and ammonium polyphosphate) of the preferred B component and inorganic fillers such as wollastonite, mineral fiber, zinc borate, etc. to synergize with solvent-free epoxy resin, which can form a dense and expanded carbon layer on the burning surface of the power battery, thereby effectively preventing the transfer of heat and the overflow of flames during the combustion process. Among them, melamine and ammonium polyphosphate are typical gas sources and acid sources in fire-retardant coatings, wollastonite and mineral fibers can play a role in improving the strength of the carbon layer, and zinc borate is a typical smoke suppressant. On the one hand, the solubilizer can ensure the stability of the fire-retardant coating, and on the other hand, it also has a flame retardant effect. Solvent-free epoxy resin has excellent high temperature resistance and bonding properties, and has excellent adhesion on metal materials such as aluminum and steel without adding a coupling agent. The solvent-free epoxy resin and the curing agent react during the curing process to form a dense coating. This coating has excellent water resistance and corrosion resistance, and can effectively prevent the penetration of moisture and other corrosive substances.
[0016] The fire retardant coating provided in this case for the power battery pack of new energy vehicles is an epoxy intumescent fire retardant coating with excellent fire retardant performance. It is suitable for the fire protection of the upper and lower shell (aluminum, stainless steel) structures of the power battery pack of new energy vehicles. It has good fireproof and heat insulation properties. After encountering flame combustion (1300℃), the coating thickness expands and has high strength. The cold surface temperature does not exceed 300℃ within 30min; the ASTMD257 resistance test exceeds 1.0×10 11 Ω; the leakage current of the compressive strength test is less than 1mA; it has excellent adhesion to metal materials such as aluminum and steel, and can be applied to electrophoretic coatings or applied alone on clean substrates; it has strong flexibility and toughness, which can ensure that the battery pack can maintain the super protective performance of the coating under the destructive force of vibration, swing and impact. It does not contain solvents, will not pollute the bonded surface, is non-toxic and harmless, and has a high solid content. At the same time, it has high insulation and excellent fireproof and heat insulation properties.
[0017] The fire retardant coating for the power battery pack of new energy vehicles is prepared by mixing component A and component B in a mass ratio of 1.7-1.9:1 when in use.
[0018] The fire retardant coating for the power battery pack of new energy vehicles is easy to use and only requires simple mixing of component A and component B.
[0019] The diluent is triphenyl phosphate.
[0020] The addition of triphenyl phosphate can improve the processing performance of the coating. Specifically, it can increase the fluidity and plasticity of the coating, making the coating smoother during stirring, mixing and coating. This not only helps to reduce the generation of bubbles and particles, but also improves the yield and quality of the coating. In addition, triphenyl phosphate, as a halogen-free and environmentally friendly flame retardant, is widely used in coatings to improve their flame retardant properties.
[0021] The solubilizing agent is castor oil.
[0022] Castor oil allows pigments, fillers, additives, etc. in paint to be evenly dispersed in aqueous or oil solutions. It helps to improve the quality and stability of the paint and ensure the uniformity and consistency of the paint during construction.
[0023] The liquid flame retardant additives in the A component and the B component are both tris(1-chloro-2-propyl) phosphate.
[0024] Tris(1-chloro-2-propyl) phosphate, as an organic phosphorus halogen compound flame retardant, has excellent flame retardant properties. When encountering a fire source, it can quickly decompose to produce phosphorus-containing compounds, which can form a protective film on the surface of the coating, thereby effectively preventing the further spread of the flame and protecting the substrate from damage.
[0025] The curing agent is a polyamide curing agent.
[0026] The preferred curing agent has a good curing effect with the epoxy resin, is easily available and has a low cost.
[0027] The accelerator is 2,4,6-tris(dimethylaminomethyl)phenol.
[0028] It mainly acts as a catalyst and curing accelerator in coatings, which can reduce the activation energy of chemical reactions in coating systems, thereby accelerating the reaction rate and improving production efficiency. At the same time, due to its mild and stable catalytic effect, it helps to obtain uniform and high-quality coatings.
[0029] The solvent-free epoxy resin is Nanya Electronic Materials E51.
[0030] This is a non-solvent epoxy resin suitable for non-solvent coatings. E51 contains epoxy groups in its molecular structure, which can form strong chemical bonds and thus exhibit excellent bonding properties. This allows E51 to adhere firmly to the surface of the substrate in the coating and is not easy to peel off or crack. This makes the coating suitable for a variety of metal and non-metal surfaces.
[0031] The method for preparing the fire retardant coating for the power battery pack of a new energy vehicle comprises the following steps:
[0032] (1) Preparation of component A:
[0033] ① At 23-25°C, add solvent-free epoxy resin, liquid flame retardant additive, solubilizer and diluent into a mixer, turn on the mixer, adjust the speed to 1000-2000 rpm, and then stir and mix for 60-90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0034] ② Then, keep the rotation speed, continue to add solid flame retardant additives, wollastonite, mineral fiber and zinc borate, and then stir and mix intermittently 3-4 times at a frequency of 60-90 seconds / time, with an interval of at least 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C to obtain a mixture;
[0035] ③ The mixture obtained in step ② is mixed in a three-roll mill until there are no obvious particles in the mixture, thereby obtaining component A;
[0036] (2) Preparation of component B:
[0037] ① At 23-25°C, add the curing agent, accelerator and liquid flame retardant additive into the mixer, turn on the mixer, adjust the speed to 1000-2000rpm, and then stir and mix for 60-90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0038] ②Then, maintain the rotation speed and continue to add solid flame retardant additives, and then stir and mix intermittently for 3-4 times at a frequency of 60-90 seconds / time, with an interval of at least 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, that is, component B is obtained.
[0039] In the preparation process of the fire retardant coating used for the power battery pack of new energy vehicles in this case, there is no dissolution difficulty problem described in the patents CN111100526A and CN 115260817A. The present invention adopts lower energy consumption to make the solid and liquid raw materials mix evenly. At the same time, the fire retardant coating used for the battery pack of new energy vehicles has high insulation, high adhesion, excellent fireproof and heat insulation performance, corrosion resistance, salt spray resistance, aging resistance and other properties. Moreover, the production process used is simple, the equipment is conventional, and it is easy to operate and implement, which is conducive to industrialized scale-up production. The mixer is preferably a self-rotating revolution mixer, and the stirring speed is the revolution speed, and the preparation efficiency is higher. That is, the preparation method of the fire retardant coating for the power battery pack of new energy vehicles is simple, the production process has low energy consumption, and it can be placed for a long time without precipitation.
[0040] The method for preparing the fire retardant coating for the power battery pack of a new energy vehicle also includes step (3) preparing the fire retardant coating for the power battery pack of a new energy vehicle: mixing component A and component B in a mass ratio of 1.7-1.9:1 to obtain the fire retardant coating for the power battery pack of a new energy vehicle.
[0041] The fire retardant coating for the power battery pack of new energy vehicles is easy to use and only requires simple mixing of component A and component B.
[0042] Compared with the prior art, the present invention has the following advantages:
[0043] 1) The fire retardant coating for the power battery pack of new energy vehicles of the present application adopts solvent-free epoxy resin to replace the water-based epoxy resin emulsion commonly used in the existing fire retardant coating, and is combined with liquid flame retardant and solubilizer, and the solid flame retardant additive, inorganic filler and epoxy resin are synergistically enhanced, which has the advantages of homogeneity, no sedimentation and excellent fire retardant performance;
[0044] 2) The fire retardant coating for the power battery pack of new energy vehicles is easy to use and only requires simple mixing of component A and component B;
[0045] 3) The preparation method of the fire retardant coating used for the power battery pack of new energy vehicles is simple, the production process has low energy consumption, and it can be placed for a long time without precipitation. The prepared fire retardant coating has the advantages of being homogeneous, free of sedimentation, high in insulation, and excellent in fireproof and heat-insulating properties. DETAILED DESCRIPTION
[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments.
[0047] The reaction system of a fire retardant coating for a new energy vehicle power battery pack described in Examples 1-3 is as follows:
[0048] Table 2 Reaction system of Examples 1-3
[0049]
[0050] Example 1
[0051] The method for preparing a fire retardant coating for a new energy vehicle power battery pack according to the present invention comprises the following steps:
[0052] (1) Preparation of component A:
[0053] ① At 23°C, add solvent-free epoxy resin, liquid flame retardant additive, solubilizer and diluent into a mixer, turn on the mixer, adjust the speed to 2000 rpm, and then stir and mix for 60 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0054] ② Then, keep the rotation speed, continue to add solid flame retardant additives, wollastonite, mineral fiber and zinc borate, and then stir and mix intermittently 3 times at a frequency of 90 seconds / time, with an interval of 6 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, to obtain a mixture;
[0055] ③ The mixture obtained in step ② is mixed in a three-roll mill until there are no obvious particles in the mixture, thereby obtaining component A;
[0056] (2) Preparation of component B:
[0057] ① At 25°C, add the curing agent, accelerator and liquid flame retardant additive into the mixer, turn on the mixer, adjust the speed to 1000 rpm, and then stir and mix for 90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0058] ②Then, maintain the rotation speed, continue to add solid flame retardant additives ammonium polyphosphate and solid flame retardant additive melamine, and then stir and mix intermittently 4 times at a frequency of 60 seconds / time, with an interval of 6 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, that is, component B is obtained.
[0059] (3) Preparation of fire retardant coatings for new energy vehicle power battery packs:
[0060] The component A and the component B are evenly mixed in a mass ratio of 1.9:1 to obtain a fire retardant coating for a power battery pack of a new energy vehicle.
[0061] Example 2
[0062] The method for preparing a fire retardant coating for a new energy vehicle power battery pack according to the present invention comprises the following steps:
[0063] (1) Preparation of component A:
[0064] ① At 24°C, add solvent-free epoxy resin, liquid flame retardant additive, solubilizer and diluent into a mixer, turn on the mixer, adjust the speed to 1500 rpm, and then stir and mix for 80 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0065] ② Then, keep the rotation speed, continue to add solid flame retardant additives, wollastonite, mineral fiber and zinc borate, and then stir and mix intermittently for 3 times at a frequency of 80 seconds / time, with an interval of 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, to obtain a mixture;
[0066] ③ The mixture obtained in step ② is mixed in a three-roll mill until there are no obvious particles in the mixture, thereby obtaining component A;
[0067] (2) Preparation of component B:
[0068] ① At 24°C, add the curing agent, accelerator and liquid flame retardant additive into the mixer, turn on the mixer, adjust the speed to 1500 rpm, and then stir and mix for 80 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0069] ②Then, maintain the rotation speed, continue to add solid flame retardant additives ammonium polyphosphate and solid flame retardant additive melamine, and then stir and mix intermittently 4 times at a frequency of 80 seconds / time, with an interval of 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, that is, component B is obtained.
[0070] (3) Preparation of fire retardant coatings for new energy vehicle power battery packs:
[0071] The component A and the component B are evenly mixed in a mass ratio of 1.8:1 to obtain a fire retardant coating for a power battery pack of a new energy vehicle.
[0072] Example 3
[0073] The method for preparing a fire retardant coating for a new energy vehicle power battery pack according to the present invention comprises the following steps:
[0074] (1) Preparation of component A:
[0075] ① At 25°C, add solvent-free epoxy resin, liquid flame retardant additive, solubilizer and diluent into a mixer, turn on the mixer, adjust the speed to 1000 rpm, and then stir and mix for 90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0076] ② Then, while maintaining the rotation speed, continue to add solid flame retardant additive, wollastonite, mineral fiber and zinc borate, and then stir and mix intermittently 4 times at a frequency of 60 seconds / time, with an interval of 8 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, to obtain a mixture;
[0077] ③ The mixture obtained in step ② is mixed in a three-roll mill until there are no obvious particles in the mixture, thereby obtaining component A;
[0078] (2) Preparation of component B:
[0079] ① At 23°C, add the curing agent, accelerator and liquid flame retardant additive into the mixer, turn on the mixer, adjust the speed to 2000 rpm, and then stir and mix for 60 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process;
[0080] ②Then, maintain the rotation speed, continue to add solid flame retardant additives ammonium polyphosphate and solid flame retardant additive melamine, and then stir and mix intermittently for 3 times at a frequency of 90 seconds / time, with an interval of 8 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, that is, component B is obtained.
[0081] (3) Preparation of fire retardant coatings for new energy vehicle power battery packs:
[0082] The component A and the component B are evenly mixed in a mass ratio of 1.7:1 to obtain a fire retardant coating for a power battery pack of a new energy vehicle.
[0083] Raw materials and equipment information involved in each embodiment:
[0084] Solvent-free epoxy resin: Brand E51, produced by Nanya Electronic Materials (Kunshan) Co., Ltd.
[0085] Curing agent: brand G-650 / G-651, produced by Guodu Chemical (Kunshan) Co., Ltd.
[0086] Solid flame retardant additives: ammonium polyphosphate, melamine, brand JLS-APP, produced by Hangzhou Jieersi Flame Retardant Chemical Co., Ltd.
[0087] Triphenyl phosphate, triisobutyl phosphate: produced by Rudong Tongyuan Chemical Co., Ltd.;
[0088] Castor oil: produced by Denghao Chemical Co., Ltd.;
[0089] Wollastonite: brand Ts320, produced by Jilin Province Lishu Dadingshan Wollastonite Co., Ltd.;
[0090] Zinc borate: produced by Shenlong Zinc Industry Co., Ltd.
[0091] Mineral fiber: produced by Hebei Hengguang Mineral Products Co., Ltd.;
[0092] Tris(1-chloro-2-propyl) phosphate: produced by Jiangsu Yak Technology Co., Ltd.;
[0093] Accelerator: 2,4,6-tris(dimethylaminomethyl)phenol, brand K54, produced by Changzhou Shanfeng Chemical Co., Ltd.
[0094] Mixer: Rotation and revolution mixer, ARE-130, THINKY.
[0095] Experimental data:
[0096] Comparative Examples 1-3: All were obtained by adjusting the control variables according to Example 2. In Comparative Example 1, the epoxy resin was replaced by water-based epoxy emulsion in equal amounts, and the process was the same as that of Example 2; in Comparative Example 2, the liquid flame retardant additive was replaced by diluent in equal amounts, and the process was the same as that of Example 2; in Comparative Example 3, the solubilizer was replaced by mineral fiber in equal amounts, and the process was the same as that of Example 2. The specific reaction system is as follows:
[0097] Table 3 Comparative Examples 1-3 Reaction System
[0098]
[0099] The fire retardant coating samples of Examples 1 to 3 and Comparative Examples 1 to 3 of the present case were subjected to performance tests.
[0100] The detection method is as follows:
[0101] The dry film thickness is controlled to be 0.6-0.9mm, and the substrate is a 0.8mm thick electrophoresis plate;
[0102] Leakage current test: Tested according to HG / T 3330-2012;
[0103] Insulation test: Tested according to GB / T1410-006 / IEC60093:1980.
[0104] The test results are as follows:
[0105] Table 1 Performance test results of each sample
[0106]
[0107] As can be seen from Table 1, the raw materials of Examples 1 to 3 of the present case have good miscibility, and the insulation performance, fire resistance and foaming performance are all good, among which Example 2 has the best comprehensive performance. Compared with Example 2, the sample of Comparative Example 1 cannot be mixed evenly, and it is meaningless to test each performance; the sample of Comparative Example 2 can be mixed evenly, but the fire resistance performance is significantly reduced; the sample of Comparative Example 3 is mixed well, but the miscibility effect is not as good as that of Example 2, and its insulation performance, fire resistance and foaming performance are all good, but there is cracking on the surface of the expansion layer.
Claims
1. A fire retardant coating for new energy vehicle power battery packs, Features: The fire retardant coating for the new energy vehicle power battery pack includes the following component A and component B: Wherein, the A component is mainly prepared from the following components in the following weight ratios: The B component is mainly prepared from the following components in the following weight ratios: The solid flame retardant additive in component A is ammonium polyphosphate, and the solid flame retardant additive in component B is a combination of ammonium polyphosphate and melamine in any proportion.
2. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The fire retardant coating for the power battery pack of new energy vehicles is prepared by mixing component A and component B in a mass ratio of 1.7-1.9:1 when in use.
3. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The diluent is triphenyl phosphate.
4. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The solubilizing agent is castor oil.
5. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The liquid flame retardant additives in the A component and the B component are both tris(1-chloro-2-propyl) phosphate.
6. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The curing agent is a polyamide curing agent.
7. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The accelerator is 2,4,6-tris(dimethylaminomethyl)phenol.
8. The fire retardant coating for a new energy vehicle power battery pack according to claim 1, Features: The solvent-free epoxy resin is Nanya Electronic Materials E51.
9. A method for preparing a fire retardant coating for a power battery pack of a new energy vehicle according to any one of claims 1 to 8, Features: The following steps are involved: (1) Preparation of component A: ① At 23-25°C, add solvent-free epoxy resin, liquid flame retardant additive, solubilizer and diluent into a mixer, turn on the mixer, adjust the speed to 1000-2000 rpm, and then stir and mix for 60-90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process; ② Then, keep the rotation speed, continue to add solid flame retardant additives, wollastonite, mineral fiber and zinc borate, and then stir and mix intermittently 3-4 times at a frequency of 60-90 seconds / time, with an interval of at least 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C to obtain a mixture; ③ The mixture obtained in step ② is mixed in a three-roll mill until there are no obvious particles in the mixture, thereby obtaining component A; (2) Preparation of component B: ① At 23-25°C, add the curing agent, accelerator and liquid flame retardant additive into the mixer, turn on the mixer, adjust the speed to 1000-2000rpm, and then stir and mix for 60-90 seconds, and ensure that the temperature is ≤80°C during the stirring and mixing process; ②Then, maintain the rotation speed and continue to add solid flame retardant additives, and then stir and mix intermittently for 3-4 times at a frequency of 60-90 seconds / time, with an interval of at least 5 minutes between two adjacent stirring and mixing to ensure that the temperature during the stirring and mixing process is ≤80°C, that is, component B is obtained.
10. The method for preparing the fire retardant coating for the power battery pack of new energy vehicles according to claim 9, Features: The method for preparing the fire retardant coating for the power battery pack of a new energy vehicle also includes step (3) preparing the fire retardant coating for the power battery pack of a new energy vehicle: mixing component A and component B in a mass ratio of 1.7-1.9:1 to obtain the fire retardant coating for the power battery pack of a new energy vehicle.
Citation Information
Patent Citations
Intumescent composition comprising a silicate modifed epoxy resin
CN107109106A
Solvent-free thick coating type epoxy resin fireproof paint and preparation method thereof
CN108264823A
The paint composition with high water-resisting and high adhesion quality necessary for steel structure painting, and its manufacturing method
KR1020130042706A
Cited By
High-viscosity low-expansion fireproof coating as well as preparation method and application thereof
CN120623873A
Fireproof flame-retardant coating for automobiles and preparation method of fireproof flame-retardant coating
CN120795725A
Fireproof coating, preparation method and application in energy storage battery
CN121249242A
Multifunctional fireproof flame-retardant coating for new energy battery and preparation method of multifunctional fireproof flame-retardant coating