Self-adhesive rubber sound insulation pad as well as preparation method and application thereof
By optimizing the rubber sound insulation layer and adhesive layer formula, combining damping fillers and odorless vulcanizers, a high-performance self-adhesive rubber sound insulation pad was developed, which solved the poor effect of floor impact sound insulation and pungent and flammable odor of traditional materials The problem of this achieves the sound insulation effect of green and environmentally friendly and convenient construction.
Patent Information
- Application Number
- CN202411235363.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
AI Technical Summary
Existing building materials have poor insulation effect on floor impact sound, and traditional sound insulation materials have problems such as pungent odor, flammable, and inconvenient construction, making it difficult to meet the sound insulation requirements of green buildings.
Use self-adhesive rubber sound insulation pads, by optimizing the formula of vulcanized rubber sound insulation layer and non-vulcanized butyl self-adhesive adhesive layer, add damping fillers such as inorganic hollow microbeads, mica powder, and use odorless vulcanizers and odor detergents. Form high-performance sound insulation materials.
It achieves high compressive strength, low compression creep, excellent impact sound insulation effect, and has no pungent odor, is convenient to construct, and meets the requirements of green and environmental protection and durability.
Smart Images

Figure BDA0005027580920000171 
Figure BDA0005027580920000181 
Figure BDA0005027580920000191
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sound insulation materials, and more specifically, relates to a self-adhesive rubber sound insulation pad and a preparation method and application thereof. Background Art
[0002] Noise pollution is the fastest growing type of pollution in modern cities, which can easily have a negative impact on human physical and mental health. With the advancement of construction technology and the improvement of people's quality of life, people are paying more and more attention to the control of environmental noise pollution, and have also put forward higher requirements for the sound insulation performance of building wall panels and floor slabs. Building sound insulation is divided into air sound insulation and impact sound insulation. For air sound insulation, sound insulation felt, shock-absorbing pads, sound-absorbing cotton, sound-absorbing panels or soundproof doors and windows can be used to effectively improve the sound insulation effect. However, for floor impact sound, since the energy of solid sound attenuates very little in traditional building materials, and the propagation speed is faster than in the air, and the propagation distance is far, the upper and lower floors are often affected by footsteps, dragging tables and chairs, running and jumping, and knocking. Continuous, hard and heavy concrete itself has a good insulation effect on airborne sound. The airborne sound insulation of a 120mm thick reinforced concrete floor can reach 48-50dB, but the insulation effect on impact sound is poor, and its impact sound pressure level is about 80-83dB, which cannot meet people's demand for reducing floor sound insulation performance, nor can it meet the relevant specifications for the sound insulation requirements of green building floors. In recent years, many national standards under preparation and revision have increased the floor impact sound pressure level indicators for floor impact sound insulation. Article 3.2.2 of the "Civil Building Sound Insulation Design Code" states: The weighted standardized impact sound pressure level of the floor between households is ≤65dB(A) for level 1, and ≤75dB(A) for levels 2 and 3.
[0003] At present, for buildings that require sound insulation, the industry mostly adopts floating design, that is, laying a layer of sound insulation material between the floating ground and the load-bearing floor to isolate the solid sound transmission effect. At present, the mainstream sound insulation materials for floating buildings are as follows: extruded polystyrene board, PU sound insulation pad, polyurethane rubber sound insulation pad, glass wool board, rock wool board, mineral wool board and ordinary rubber sound insulation pad.
[0004] Extruded polystyrene board uses polystyrene as the main material, and has an independent closed bubble structure inside. It is one of the most widely used sound insulation materials at present, with a high improvement in airborne sound, but its improvement in impact sound is poor; PU sound insulation pad is made of pure polyurethane foam, with good sound insulation effect, but the price is high, and it has large permanent deformation under long-term heavy pressure, and the sound insulation effect deteriorates; polyurethane rubber sound insulation pad is made of a mixture of polyurethane adhesive and foam, rubber particles and other materials, and the impact sound improvement can reach 15dB-20dB, but it is an adhesive product with poor comprehensive material performance, and the waste rubber particles and polyurethane adhesive added in it will deteriorate after long-term use. There is a potential environmental risk of releasing VOC gas during use; glass wool board, rock wool board, and mineral wool board are also large-volume sound insulation materials, but these three materials are rigid fiberboards. On the one hand, the fiber structure is very easy to absorb water, and on the other hand, it needs to be cut on site, which is inconvenient for construction; foam sound insulation products have problems such as large compression deformation as the use time increases; ordinary rubber sound insulation pads generally use traditional vulcanization systems for sound insulation effects. Their sound insulation effects increase with the increase of rubber content and product thickness, but due to formula design problems, most of them emit irritating sulfurized odors and are difficult to be used for laying in places with high environmental protection requirements such as residences and office buildings. In response to the above problems, it is urgent to develop a sound insulation material with high compressive strength, small compression creep, low water absorption, good impact sound isolation effect, convenient construction, green environmental protection, and excellent sound insulation durability. Summary of the invention
[0005] The purpose of the present invention is to provide a self-adhesive rubber sound insulation pad and a preparation method and application thereof. The present invention optimizes the raw material formula of the vulcanized rubber sound insulation layer so that the prepared self-adhesive rubber sound insulation pad has the characteristics of high compressive strength, small compression creep, no pungent odor, and excellent impact sound insulation effect.
[0006] In order to achieve the above-mentioned object, a first aspect of the present invention provides a self-adhesive rubber sound insulation pad, the self-adhesive rubber sound insulation pad comprising: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer;
[0007] The raw materials for preparing the vulcanized rubber sound insulation layer include: natural rubber, butyl rubber, a first filler, inorganic hollow microspheres, cork powder, a first activation processing aid, a first plasticizer, an odorless vulcanizing agent, an accelerator, an antioxidant, a deodorizing agent, optional rubber powder, an optional first flame retardant, an optional first tackifying resin, an optional anti-scorch agent and an optional release agent.
[0008] In the present invention, preferably, the non-vulcanized butyl self-adhesive adhesive layer is disposed on the vulcanized rubber sound insulation layer. Further preferably, an isolation film layer is also disposed on the non-vulcanized butyl self-adhesive adhesive layer.
[0009] In the present invention, preferably, the thickness of the vulcanized rubber sound insulation layer is 2-5 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.3-0.6 mm.
[0010] In the present invention, the rubber sound insulation pad uses natural rubber as the main material. The main component of natural rubber is cis-1,4-polyisoprene, which has few side groups in the molecular chain, small volume, low cohesive energy density, high molecular chain flexibility, and is easy to convert the mechanical energy of sound wave vibration into heat energy for dissipation. At the same time, although the damping coefficient of natural rubber is not high, its loss factor distribution is wide, and it can provide a good damping effect in a large temperature range. In the present invention, butyl rubber is added to the sound insulation layer to improve the overall sound insulation performance of the rubber. At the same time, butyl rubber has good thermoplasticity and self-adhesion, which helps to improve the dispersion effect between the rubber and the filler, and effectively improves the overall bonding molding ability and cohesive strength of the rubber; the double bond density in butyl rubber is low, which gives the material better weather resistance and durability, and its excellent high and low temperature resistance can also effectively broaden the working temperature range of the rubber sound insulation pad; in addition, the methyl distribution density of the side chain of butyl rubber is relatively large, and its steric effect can hinder the movement of rubber macromolecules, increase the internal friction between molecules, and have a higher damping coefficient and loss factor. In the present invention, by selecting natural rubber and butyl rubber with certain compatibility and co-vulcanization properties for blending, the damping peak width can be effectively widened, the loss factor can be increased, and the damping characteristics can be improved.
[0011] In the present invention, the added inorganic hollow microspheres have the advantages of light weight, low thermal conductivity, high strength and good chemical stability, and at the same time have oleophilic and hydrophobic properties, and are very easy to disperse in organic materials such as rubber and resin. The closely arranged inorganic hollow microspheres contain rarefied gas inside, and have a small specific gravity. Therefore, when they are introduced into the rubber sound insulation pad, they can not only reduce the specific gravity of the product, making it easier to carry and construct, but also their hollow gas layer can isolate sound waves, increase the reflection of sound waves, and accelerate the attenuation and consumption of sound wave energy, greatly improving the sound insulation performance. At the same time, the inorganic hollow microspheres can improve the strength, wear resistance and rigidity of the composite material.
[0012] The high-performance self-adhesive rubber sound insulation pad for floor impact prepared by the present invention comprises a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer. The sound insulation layer plays the role of vibration reduction and sound insulation, and the self-adhesive layer plays the role of good adhesion to the base floor, no displacement, sealing and waterproofing, and convenient construction.
[0013] According to the present invention, preferably, in parts by weight, relative to 100 parts of natural rubber, the butyl rubber is 10-50 parts, the rubber powder is 0-100 parts, the first filler is 150-350 parts, the first flame retardant is 0-50 parts, the inorganic hollow microspheres are 10-80 parts, the cork powder is 10-80 parts, the first activation processing aid is 3-10 parts, the first tackifying resin is 0-5 parts, the first plasticizer is 10-70 parts, the odorless vulcanizing agent is 1-5 parts, the accelerator is 1-3 parts, the scorch retarder is 0-2 parts, the antioxidant is 1-5 parts, the release agent is 0-4 parts, and the deodorizing agent is 5-20 parts.
[0014] According to the present invention, preferably, the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer include: butyl rubber, a second filler, a second activation processing aid, a second plasticizer, a second tackifying resin, an antioxidant, a light stabilizer, an optional second flame retardant and an optional polyisobutylene;
[0015] Preferably, in parts by weight, relative to 100 parts of butyl rubber, the polyisobutylene is 0-50 parts, the second filler is 50-150 parts, the second flame retardant is 0-40 parts, the second activation processing aid is 1-10 parts, the second plasticizer is 2-30 parts, the second tackifying resin is 50-200 parts, the antioxidant is 1-3 parts, and the light stabilizer is 1-3 parts.
[0016] In the present invention, it is further preferred that, based on weight parts, relative to 100 parts of butyl rubber, the polyisobutylene is 40-50 parts, the second filler is 90-130 parts, the second flame retardant is 10-30 parts, the second activation processing aid is 4-8 parts, the second plasticizer is 8-20 parts, the second tackifying resin is 80-130 parts, the antioxidant is 2-3 parts, and the light stabilizer is 1-3 parts.
[0017] According to the present invention, preferably, the first plasticizer is selected from at least one of naphthenic oil, paraffin oil, rosin oil and soybean oil;
[0018] The first tackifying resin is selected from at least one of C5 petroleum resin, C9 petroleum resin and terpene resin;
[0019] The first activation processing aid is selected from at least one of zinc oxide, stearic acid and zinc stearate;
[0020] The first flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide, phosphorus nitrogen intumescent flame retardant and intumescent graphite flame retardant;
[0021] The first filler is preferably selected from mica powder and an optional first other filler, and the first other filler is selected from at least one of carbon black, calcium carbonate, white carbon, clay and talc; further preferably, the mass ratio of the first other filler to the mica powder is (0-6):1.
[0022] In the present invention, preferably, the first filler comprises mica powder, carbon black, white carbon black and calcium carbonate. In parts by weight, the amount of mica powder is 40-60 parts, the amount of carbon black is 30-50 parts, the amount of white carbon black is 10-20 parts, and the amount of calcium carbonate is 100-150 parts.
[0023] In the present invention, the preferred addition of a variety of fillers can not only effectively reduce production costs, but also help to evenly disperse the various components of the rubber during processing and mixing, thereby improving the processability of the rubber; the addition of carbon black can fill and reinforce the rubber, giving the mixed rubber and vulcanized rubber excellent tensile strength and elongation at break; the addition of calcium carbonate can increase the volume and reduce costs while increasing the density and specific gravity of the vulcanized rubber products, which can effectively improve the sound insulation performance; the added mica powder can effectively enhance the viscoelasticity of natural rubber. When vibration or sound waves pass through, the flaky mica powder will move in the vertical direction of the vibration and sound wave propagation, generate friction with the rubber molecular chains around it, and quickly convert the vibration mechanical energy into heat energy, thereby playing a damping and vibration reduction role in a wider temperature range and lower frequency; carbon black, calcium carbonate, mica powder, and rubber molecular chains rub against each other under the action of vibration and sound waves to generate heat, playing a damping and vibration reduction role and converting mechanical energy into heat energy.
[0024] According to the present invention, preferably, the second plasticizer is selected from at least one of naphthenic oil, paraffin oil, rosin oil and soybean oil;
[0025] The second tackifying resin is selected from at least one of C5 petroleum resin, C9 petroleum resin and terpene resin;
[0026] The second activation processing aid is selected from at least one of zinc oxide, stearic acid and zinc stearate;
[0027] The second flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide, phosphorus nitrogen intumescent flame retardant and intumescent graphite flame retardant;
[0028] The second filler is preferably selected from mica powder and an optional second other filler, and the second other filler is selected from at least one of carbon black, calcium carbonate, white carbon, clay and talc; further preferably, the mass ratio of the second other filler to the mica powder is (0-6):1.
[0029] In the present invention, preferably, the second filler comprises mica powder and calcium carbonate, and the mass ratio of the calcium carbonate to the mica powder is (3-6):1.
[0030] In the present invention, inorganic hollow microspheres, optional rubber powder, cork powder and mica are introduced into the rubber filling system, and the optimal sound insulation performance is achieved through the synergistic effect of the above components and rubber. The sound insulation effect is 15 to 25 dB higher than that of traditional rubber sound insulation pad products and polyurethane sound insulation pad products of the same thickness, and the product has high compressive strength and low compression creep.
[0031] According to the present invention, preferably, the accelerator is selected from at least one of trimethylallyl isocyanate (H-2), triallyl isocyanurate (TAIC), N,N'-m-phenylene bismaleimide (HVA-2), trimethylolpropane methacrylate (TMPTMA) and p-benzoquinone dioxime (MSDS);
[0032] The scorch retarder is selected from at least one of N-cyclohexylthiophthalamide (CTP), phthalic anhydride and N-nitrosodiphenylamine (NDPA);
[0033] The antioxidant is at least one of antioxidant RD, antioxidant MB, antioxidant 4010NA and antioxidant 4020;
[0034] The rubber powder is preferably selected from at least one of 20 mesh rubber powder, 50 mesh rubber powder and 100 mesh rubber powder;
[0035] The odorless vulcanizing agent is preferably selected from at least one of benzoyl hydroperoxide, diisopropyl bis-tert-butyl peroxide (BIBP) and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane (DBPH).
[0036] In the present invention, compared with the traditional rubber sound insulation pad, the product of the present invention does not contain sulfur, uses an odorless peroxide vulcanization system, does not emit a pungent sulfur smell, is environmentally friendly and non-toxic, and does not emit VOC gases such as hydrogen sulfide, sulfur dioxide, and sulfur trioxide during use.
[0037] In the present invention, the addition of rubber powder can not only reduce the production cost, but also the large-particle rubber powder in the mixed rubber is evenly blended with the raw rubber, and the micropores formed therein can accommodate a small amount of air, which can effectively improve the comprehensive sound insulation effect of the sound insulation pad. Preferably, the rubber powder cannot be rubber powder particles recycled from waste rubber.
[0038] In the present invention, the vulcanizing agent and the accelerator can work synergistically to make the natural rubber of the sound insulation layer vulcanize quickly at high temperature, and the vulcanized rubber does not produce pungent gas. The addition of the deodorizing agent can utilize its porous structure to absorb as many small molecules produced by the vulcanization reaction as possible, thereby playing a role in deodorizing and environmental protection during long-term use.
[0039] According to the present invention, preferably, the inorganic hollow microspheres are at least one of 40 mesh hollow glass microspheres, 80 mesh hollow glass microspheres, 120 mesh hollow glass microspheres, 40 mesh hollow ceramic microspheres, 80 mesh hollow ceramic microspheres and 120 mesh hollow ceramic microspheres;
[0040] The cork powder is selected from at least one of 60-mesh cork powder, 100-mesh cork powder and 150-mesh cork powder.
[0041] According to the present invention, preferably, the weight average molecular weight of the polyisobutylene is 1300-2400;
[0042] The antioxidant is antioxidant 1010;
[0043] The light stabilizer is BASF light stabilizer 2020.
[0044] In the present invention, the second plasticizer and the optional polyisobutylene are added to soften the rubber, increase the bonding cohesion between the rubber and the filler, and improve the elongation, plasticity and flexibility of the rubber; the second plasticizer is added to reduce the Mooney viscosity of the rubber, enhance the plasticity, and facilitate calendering and extrusion processing; the second tackifying resin is added to improve the initial adhesion and sustained adhesion effect of the butyl rubber of the adhesive layer, which is helpful for sealing and bonding with the base material and improving the peel strength. Too little amount reduces the initial adhesion and sustained adhesion effect of the adhesive layer, and too much amount reduces the cohesion and temperature resistance of the colloid.
[0045] In the present invention, rubber is a macromolecular material with a large molecular volume, good molecular chain flexibility, excellent viscoelasticity and high damping properties, and is an ideal sound insulation matrix material. Traditional rubber sound insulation products are often filled with inorganic fillers such as carbon black, white carbon black, and calcium carbonate. The friction between fillers and fillers, and between fillers and rubber is limited, resulting in limited sound insulation performance. The impact sound insulation of 3mm thick sound insulation products is generally less than 15dB; and the sulfur vulcanization system is used, and vulcanization accelerators such as CZ, M, DM, and TMTD are used for processing and production. The vulcanized products have a pungent odor. The present invention designs a formula for natural rubber, uses odorless peroxide as a vulcanizing agent, and matches it with a vulcanization accelerator, thereby greatly reducing the pungent smell generated by vulcanization, achieving the production of odorless rubber products, and being low-carbon, environmentally friendly, and free of VOC gas emissions, meeting the requirements of indoor sound insulation application scenarios; at the same time, the present invention preferably introduces three raw materials, namely, mica powder, cork powder, and inorganic hollow microspheres, and utilizes the lamellar structure of mica powder, the sound absorption of cork powder, and the sound insulation of inorganic hollow microspheres. Through effective proportioning and the synergistic effect of the three raw materials, the internal friction effect of the material under the action of sound wave vibration is increased, and the sound wave damping effect of the rubber composite material at different frequencies is improved, so that the excellent sound insulation performance of 3mm thick rubber products up to 25dB to 35dB is achieved.
[0046] In the present invention, preferably, the high-performance odorless self-adhesive rubber sound insulation pad of the present invention uses natural rubber and environmentally friendly rubber powder as the main materials, supplemented by inorganic fillers such as carbon black, white carbon black, calcium carbonate, etc., so that the sound insulation pad has good mechanical properties and elasticity; the introduction of high loss factor butyl rubber gives it good sound insulation performance, and at the same time helps to effectively improve the overall bonding molding ability and cohesive strength of the rubber; the introduction of mica powder effectively enhances the viscoelasticity of natural rubber, and its lamellar structure and the internal friction with other inorganic fillers and rubber molecular chains can quickly convert the mechanical energy of sound wave vibration into heat energy, thereby playing a damping and vibration reduction role in a wider temperature range and lower frequency. Use; The introduction of inorganic hollow microspheres can increase the reflection of sound waves, accelerate the attenuation and consumption of sound wave energy, and synergize with inorganic fillers such as mica to significantly improve the sound insulation performance. At the same time, inorganic hollow microspheres can improve the strength, wear resistance and rigidity of composite materials; The introduction of flame retardants can change the flammable properties of rubber, and effectively prevent, delay or terminate the spread of flames when the material burns; The synergistic effect of odorless vulcanizers and accelerators allows natural rubber to vulcanize quickly at high temperatures, and the vulcanized rubber does not produce pungent gases; The addition of deodorizers can utilize their porous structure to absorb as many small molecules produced by the vulcanization reaction as possible, and play a role in deodorizing and environmental protection during long-term use.
[0047] In the present invention, preferably, by introducing mica powder, cork powder, rubber powder particles, inorganic hollow microspheres and other damping fillers, through effective proportioning and synergistic effect, the optimal impact sound insulation performance is achieved, so that it has excellent damping sound insulation for sound waves of different frequencies under different temperature environments, and its impact sound improvement is as high as 20-35dB, which is much higher than the sound insulation material of the same thickness. At the same time, the butyl self-adhesive layer of the product can not only be firmly bonded to various substrates such as concrete, metal plates, and wood to achieve effective sealing and waterproofing, but also enhance the sound insulation and shock absorption performance. Its bonding and paving without displacement can effectively improve the convenience of construction. In addition, its good flame retardancy also improves its safety in use.
[0048] In the present invention, the high-performance flame-retardant self-adhesive rubber sound insulation pad for floor impact prepared by the present invention can effectively solve the problems of poor sound insulation effect of floor impact of existing sound insulation materials, pungent odor, flammable materials, inconvenient construction, etc.
[0049] The second aspect of the present invention provides a method for preparing the self-adhesive rubber sound insulation pad, the method comprising:
[0050] (1) putting the natural rubber, butyl rubber and optional rubber powder into an internal mixer for internal mixing, then putting a first activated processing aid, an antioxidant, a deodorant, an optional first tackifying resin and an optional release agent into the internal mixer for internal mixing, and finally putting a first filler, inorganic hollow microspheres, cork powder, a first plasticizer and an optional first flame retardant into the internal mixer for internal mixing, and then removing the rubber;
[0051] (2) placing the rubber material obtained in step (1) on an open mixing mill for mixing to obtain a mixed rubber;
[0052] (3) putting the first-stage mixed rubber obtained in step (2) into an internal mixer for internal mixing, and then adding the odorless vulcanizing agent, accelerator and optional scorch retarder, and performing internal mixing and rubber removal;
[0053] (4) placing the rubber material obtained in step (3) on an open mixing mill for mixing to obtain a two-stage mixed rubber;
[0054] (5) the two-stage mixed rubber obtained in step (4) is made into a rubber coil in a screw extruder, and then the rubber coil is calendered and vulcanized at 160-170° C. on a drum vulcanizer to obtain the vulcanized rubber sound insulation layer;
[0055] (6) mixing the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer in an internal mixer to remove the adhesive;
[0056] (7) Extrusion coating the self-adhesive rubber obtained in step (6) on the vulcanized rubber sound insulation layer to form a self-adhesive rubber layer, and then calendering it through a double-roll calender to obtain the self-adhesive rubber sound insulation pad.
[0057] In the present invention, preferably, in step (7), before calendering by a double-roll calender, a release protective film is applied on the self-adhesive layer, and then calendering by a double-roll calender is performed to obtain the self-adhesive rubber sound insulation pad.
[0058] In the present invention, as a preferred embodiment, the preparation method of the present invention comprises the following steps:
[0059] (1) putting the natural rubber, butyl rubber and optional rubber powder into an internal mixer and kneading them at 90-110° C. for 5-10 min, then putting the first activation processing aid, antioxidant, deodorant, optional first tackifying resin and optional release agent into the internal mixer and kneading them at 115-130° C. for 5-10 min, finally putting the first filler, inorganic hollow microspheres, cork powder, first plasticizer and optional first flame retardant into the internal mixer and kneading them at 115-130° C. for 10-15 min or until the kneading temperature reaches 140° C., and then removing the glue;
[0060] (2) placing the rubber material obtained in step (1) on an open mill for open milling to obtain a first-stage mixed rubber; more preferably, placing the rubber material obtained in step (1) on an open mill, thinly packing the rubber material, the first-stage mixing roller distance is 3-4 mm, and the rubber material is placed on a plate 3 times; the second-stage mixing is performed to adjust the thickness of the rubber sheet to 8±2 mm, and 3 / 4 rubber tapping is performed 6 times to obtain a first-stage mixed rubber; the first-stage mixed rubber is parked for ≥8 hours before the second-stage mixing process is performed;
[0061] (3) the first-stage mixed rubber obtained in step (2) is put into an internal mixer and mixed at 60-80° C. for 3-5 min, and then the odorless vulcanizing agent, accelerator and optional anti-scorching agent are added, mixed for 5-10 min, and the rubber is discharged; in this step, the temperature of the internal mixer should be strictly controlled not to be higher than 100° C. to prevent the rubber from scorching;
[0062] (4) placing the rubber obtained in step (3) on an open mill for open milling to obtain a two-stage mixed rubber; more preferably, placing the rubber obtained in step (3) on an open mill, thinly packing, the first open milling roll distance is 3-4 mm, and the rubber is placed on a plate 3 times; the second open milling adjusts the rubber sheet thickness to 8±2 mm, performs 3 / 4 rubber tapping 6 times, and obtains a two-stage mixed rubber; the second-stage mixed rubber is left for ≥8 hours before the subsequent vulcanization process is carried out;
[0063] (5) Extruding the two-stage mixed rubber obtained in step (4) into a rubber coil in a screw extruder, and then calendering and vulcanizing the rubber coil on a drum vulcanizer at 160-170° C. to obtain the vulcanized rubber sound insulation layer; wherein, preferably, the extrusion temperature of the rubber coil in the screw extruder is preferably 60-70° C.; and the calendering and vulcanization pressure is 3-6 MPa;
[0064] (6) kneading the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer in an internal mixer for 20-40 minutes to 120-140° C. to remove the adhesive;
[0065] (7) Extrusion coating the self-adhesive rubber obtained in step (6) on the vulcanized rubber sound insulation layer to form a self-adhesive rubber layer, and then calendering it through a double-roll calender to obtain the self-adhesive rubber sound insulation pad; wherein, preferably, the extrusion coating temperature is 120-140°C.
[0066] The third aspect of the present invention provides the use of the self-adhesive rubber sound insulation pad as a vibration-damping sound insulation pad for a floating floor of a building.
[0067] The technical solution of the present invention has the following beneficial effects:
[0068] (1) The present invention optimizes the raw material formula of the vulcanized rubber sound insulation layer, so that the prepared self-adhesive rubber sound insulation pad has the characteristics of high compressive strength, small compression creep, no pungent odor, and excellent impact sound insulation effect.
[0069] (2) The self-adhesive rubber sound insulation pad of the present invention uses natural rubber with excellent comprehensive performance as the main material. On the one hand, the vulcanization system is improved. By selecting specific odorless vulcanizing agents and accelerators, the odor generated by the vulcanization process is significantly reduced, and no VOC toxic gases are generated, meeting the requirements of environmentally friendly and non-toxic indoor use; on the other hand, by optimizing the raw material formula of the vulcanized rubber sound insulation layer, the prepared self-adhesive rubber sound insulation pad has the characteristics of high compressive strength, small compression creep, and excellent impact sound insulation effect.
[0070] (3) The self-adhesive rubber sound insulation pad of the present invention is a soft rubber coil, which can be poured with mortar after being laid flat, and the construction is convenient. Its good mechanical properties, sound insulation effect, flame retardancy and green environmental protection characteristics enable it to meet the use requirements of the vibration reduction and sound insulation pad of the floating floor of the building.
[0071] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0072] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0073] The present invention is further described below by examples:
[0074] In the following embodiments and comparative examples:
[0075] The rubber powder is 20 mesh, purchased from Jiangmen Pinxi New Materials Co., Ltd., with the brand name B20; the terpene resin is purchased from Puyang Hengfeng Petrochemical Co., Ltd., with the brand name FST-TR100; the mold release agent is purchased from Wuxi Binwang Chemical Plant, with the brand name FS-12A; the deodorant is purchased from Ningbo Jiahe New Materials Technology Co., Ltd., with the brand name JH-100A; the expanded graphite flame retardant is purchased from Shanghai Youmo Composite Materials Co., Ltd., with the brand name PX; polyisobutylene is purchased from Dalin, South Korea, with the brand name PB-1400 and the weight average molecular weight of 1400; the light stabilizer is BASF light stabilizer 2020;
[0076] The particle size of mica powder is 400 mesh; the particle size of carbon black is 45um, the particle size of white carbon black is 800 mesh, and the particle size of calcium carbonate is 600 mesh.
[0077] Examples 1-5
[0078] This embodiment provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0079] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0080] In parts by weight, the raw materials for preparing the non-vulcanized butyl self-adhesive bonding layer include: 100 parts of butyl rubber, 50 parts of polyisobutylene with a weight average molecular weight of 1400, 80 parts of calcium carbonate, 20 parts of mica powder, 15 parts of magnesium hydroxide flame retardant, 6 parts of zinc stearate, 10 parts of paraffin oil, 100 parts of terpene resin, 3 parts of antioxidant 1010, and 2 parts of light stabilizer 2020.
[0081] The specific preparation method of the self-adhesive rubber sound insulation pad of this embodiment is as follows:
[0082] 1. Preparation of vulcanized rubber sound insulation layer
[0083] (1) Preparation of a rubber compound
[0084] Natural rubber, butyl rubber and optional rubber powder calculated by weight are put into an internal mixer and kneaded at 100°C for 8 minutes. Subsequently, the first activated processing aid zinc stearate, terpene resin, antioxidant 4010NA, release agent and deodorant are put into an internal mixer and kneaded at 120°C for 8 minutes. After mixing evenly, carbon black, white carbon black, calcium carbonate, optional mica powder, 40-mesh hollow glass microspheres, 100-mesh cork powder, optional expanded graphite flame retardant and paraffin oil are put into an internal mixer and continue to knead at 120°C for 13 minutes to discharge the rubber.
[0085] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the first-stage mixed rubber. The first-stage mixed rubber can be carried out only after it has been parked for ≥8h before the second-stage mixing process.
[0086] (2) Preparation of two-stage rubber compound
[0087] Put the cooled rubber mixture into the internal mixer and mix it at 70℃ for 4 minutes, then add the odorless vulcanizer BIBP and accelerator MSDS, mix it for 8 minutes and discharge the rubber. In this step, the temperature of the internal mixer should be strictly controlled not to be higher than 100℃ to prevent the rubber from burning.
[0088] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the second-stage mixed rubber. The second-stage mixed rubber can only be used for the subsequent vulcanization process after it has been parked for ≥8h.
[0089] (3) Rubber coil vulcanization
[0090] Feed the rubber (two-stage mixed rubber) into a screw extruder, set the extrusion temperature to 70°C, and make the rubber into a rubber coil of specified thickness; then place the rubber coil on a drum vulcanizer, and use a high-temperature calendering roller to calender and vulcanize it at 160°C and 5MPa pressure to obtain a vulcanized rubber coil (vulcanized rubber sound insulation layer), which can be used as the sound insulation layer of a self-adhesive rubber sound insulation pad and can be stored after being rolled up.
[0091] 2. Preparation of butyl self-adhesive
[0092] Put 100 parts of butyl rubber, 50 parts of polyisobutylene with a weight average molecular weight of 1400, 80 parts of calcium carbonate, 20 parts of mica powder, 15 parts of magnesium hydroxide flame retardant, 6 parts of zinc stearate, 10 parts of paraffin oil, 100 parts of terpene resin, 3 parts of antioxidant 1010 and 2 parts of light stabilizer 2020 into an internal mixer and mix for 30 minutes, until the temperature reaches 130°C for debonding, and then seal and store for later use.
[0093] 3. Preparation of self-adhesive rubber sound insulation pads
[0094] Put the butyl self-adhesive adhesive into a single-screw extruder, extrusion-coat it on the vulcanized rubber sound insulation layer at 130°C to form a self-adhesive adhesive layer, apply a release protective film on the self-adhesive adhesive layer, calender it through a double-roll calender, and roll it up to obtain a self-adhesive rubber sound insulation pad.
[0095] Comparative Example 1
[0096] This comparative example provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0097] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0098] The specific formula of the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer is the same as that in Example 1;
[0099] The preparation method of the self-adhesive rubber sound insulation pad of this comparative example is different from that of Example 1 only in that when preparing a first-stage mixed rubber, no deodorizing agent is added during the mixing; the other process steps and process conditions are the same as those of Example 1.
[0100] Comparative Example 2
[0101] This comparative example provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0102] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0103] The specific formula of the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer is the same as that in Example 1;
[0104] The preparation method of the self-adhesive rubber sound insulation pad of this comparative example is different from that of Example 1 only in that when preparing a first-stage mixed rubber, 40-mesh hollow glass microspheres are not added during the banburying; the other process steps and process conditions are the same as those of Example 1.
[0105] Comparative Example 3
[0106] This comparative example provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0107] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0108] The specific formula of the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer is the same as that in Example 1;
[0109] The preparation method of the self-adhesive rubber sound insulation pad of this comparative example is different from that of Example 1 only in that when preparing a first-stage mixed rubber, no 100-mesh cork powder is added during the banburying; the other process steps and process conditions are the same as those of Example 1.
[0110] Comparative Example 4
[0111] This comparative example provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0112] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0113] The specific formula of the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer is the same as that in Example 1;
[0114] The preparation method of the self-adhesive rubber sound insulation pad of this comparative example differs from that of Example 1 only in the following aspects:
[0115] (1) Preparation of a rubber compound
[0116] Natural rubber, butyl rubber and rubber powder calculated by weight were put into an internal mixer and kneaded at 100°C for 8 minutes. Subsequently, the first activated processing aid zinc stearate, terpene resin, antioxidant 4010NA and release agent were put into an internal mixer and kneaded at 120°C for 8 minutes. After mixing evenly, carbon black, white carbon black, calcium carbonate, mica powder, 40 mesh hollow glass microspheres, 100 mesh cork powder, expanded graphite flame retardant and paraffin oil were put into an internal mixer and continued to knead at 120°C for 13 minutes to discharge the rubber.
[0117] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the first-stage mixed rubber. The first-stage mixed rubber can be carried out only after it has been parked for ≥8h before the second-stage mixing process.
[0118] (2) Preparation of two-stage rubber compound
[0119] Put the cooled rubber mixture into the internal mixer and mix it at 70℃ for 4 minutes. Then add sulfur, accelerator TT and anti-scorch agent CTP, mix it for 8 minutes and discharge the rubber. In this step, the temperature of the internal mixer should be strictly controlled not to be higher than 100℃ to prevent the rubber from scorching.
[0120] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the second-stage mixed rubber. The second-stage mixed rubber can only be used for the subsequent vulcanization process after it has been parked for ≥8h.
[0121] The other process steps and process conditions are the same as those in Example 1.
[0122] Comparative Example 5
[0123] This comparative example provides a self-adhesive rubber sound insulation pad, which includes: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; wherein the thickness of the vulcanized rubber sound insulation layer is 3 mm, and the thickness of the non-vulcanized butyl self-adhesive adhesive layer is 0.5 mm;
[0124] The specific formula of the raw materials for preparing the vulcanized rubber sound insulation layer is shown in Table 1;
[0125] The specific formula of the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer is the same as that in Example 1;
[0126] The preparation method of the self-adhesive rubber sound insulation pad of this comparative example differs from that of Example 1 only in the following aspects:
[0127] (1) Preparation of a rubber compound
[0128] Natural rubber and butyl rubber calculated by weight were put into an internal mixer and kneaded at 100°C for 8 minutes. Subsequently, the first activated processing aid zinc stearate, terpene resin, antioxidant 4010NA and release agent were put into an internal mixer and kneaded at 120°C for 8 minutes. After mixing evenly, carbon black, white carbon black, calcium carbonate and paraffin oil were put into the internal mixer and continued to knead at 120°C for 13 minutes to discharge the rubber.
[0129] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the first-stage mixed rubber. The first-stage mixed rubber can be carried out only after it has been parked for ≥8h before the second-stage mixing process.
[0130] (2) Preparation of two-stage rubber compound
[0131] Put the cooled rubber mixture into the internal mixer and mix it at 70℃ for 4 minutes. Then add sulfur, accelerator TT and anti-scorch agent CTP, mix it for 8 minutes and discharge the rubber. In this step, the temperature of the internal mixer should be strictly controlled not to be higher than 100℃ to prevent the rubber from scorching.
[0132] Place the rubber obtained in the previous step on the open mill, pack it thinly, and roll it 4mm in the first open mill, and put it on the plate 3 times; adjust the thickness of the rubber sheet to 8±2mm in the second open mill, and perform 3 / 4 rubber tapping 6 times to obtain the second-stage mixed rubber. The second-stage mixed rubber can only be used for the subsequent vulcanization process after it has been parked for ≥8h.
[0133] The other process steps and process conditions are the same as those in Example 1.
[0134] Table 1
[0135]
[0136]
[0137] Test Case
[0138] The above-mentioned embodiments and comparative examples were subjected to performance tests, and the specific test methods are as follows; the specific test results are shown in Table 3.
[0139] Among them, test 1: tensile properties
[0140] The tensile strength (MPa) of the vulcanized rubber sound insulation layer prepared in each embodiment and each comparative example was tested according to GB / T 528-2009 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”.
[0141] Test 2: Tearing performance
[0142] The tear strength (N / mm) of the vulcanized rubber sound insulation layer prepared in each embodiment and each comparative example was tested according to GB / T 529-2008 “Determination of tear strength of vulcanized rubber or thermoplastic rubber”.
[0143] Test 3: Hardness
[0144] The Shore hardness of the vulcanized rubber sound insulation layer prepared in each embodiment and each comparative example was tested according to GB / T 531.1-2008 “Test method for indentation hardness of vulcanized rubber or thermoplastic rubber”.
[0145] Test 4: Compression set
[0146] According to GB / T 7759.1-2015 “Determination of permanent compression set of vulcanized rubber or thermoplastic rubber”, the elasticity retention capacity of the vulcanized rubber sound insulation layer prepared in each embodiment and each comparative example after continuous compression at room temperature was tested.
[0147] Test 5: Combustion Performance
[0148] The combustion performance grade of the self-adhesive rubber sound insulation pads prepared in each embodiment and comparative example was tested according to GB / T 8624-2012 "Combustion Performance Classification of Building Materials and Products".
[0149] Test 6: Waterproofness
[0150] According to GB / T 328.10-2007 "Test methods for building waterproof membranes Part 10 Waterproofness of bitumen and polymer waterproof membranes", the water pressure resistance and water impermeability of the self-adhesive rubber sound insulation pads prepared in each embodiment and comparative example were tested.
[0151] Test 7: Peel Strength
[0152] The peeling strength between the self-adhesive rubber sound insulation pads prepared in each embodiment and comparative example and the cement mortar board was tested according to GB / T 328.21-2007 "Test methods for building waterproof membranes Part 21: Peeling properties of polymer waterproof membrane joints".
[0153] Test 8: Odor Rating
[0154] Five operators were invited to evaluate the odor produced by the self-adhesive rubber sound insulation pads according to the Japanese odor classification method. The odor intensity classification is shown in the following table.
[0155] Table 2. Rubber odor intensity classification standard
[0156]
[0157] Test 9: Release of Hazardous Substances
[0158] According to GB 18583-2008 “Harmful substances in adhesives for interior decoration and furnishing materials”, the contents of benzene, toluene + xylene (g / kg) of the vulcanized rubber sound insulation layer prepared in each embodiment and comparative example were tested.
[0159] According to GB 18587-2001 "Limits of harmful substances released from carpets, carpet padding agents and carpet adhesives for interior decoration and renovation materials", the total volatile organic compounds and formaldehyde contents (mg / m 2 h).
[0160] Test 10: Floor impact sound insulation performance
[0161] Clean the floor to be constructed and keep it clean and dry. Then tear off the release protective film of the self-adhesive rubber sound insulation pad, stick the self-adhesive colloid layer directly on the structural floor, and use a roller to remove the bubbles on the surface; then pour a 35mm thick fine stone concrete protective layer on top of the rubber sound insulation pad. After the fine stone concrete protective layer is completely cured, carry out the floor impact sound insulation performance test according to the GB / T 50121-2005 standard method.
[0162] According to GB / T 50121-2005 "Building Sound Insulation Evaluation Standard", the normalized impact sound pressure level of the reference floor with a weighted normalized impact sound pressure level of 78 dB is tested for the normalized impact sound pressure level of the self-adhesive rubber sound insulation pads prepared in each embodiment and the comparative example at different impact frequencies, and the normalized impact sound pressure level improvement is represented by the impact sound pressure level improvement ΔL.
[0163] Table 3
[0164]
[0165]
[0166] According to the results in Table 3, the introduction of damping fillers such as mica powder, hollow glass beads, rubber powder particles and cork powder can significantly improve the impact sound insulation effect of the floor slab. The introduction of flame retardant fillers can effectively improve the flame retardant properties. The introduction of odorless vulcanization system and rubber deodorizer can significantly reduce the odor of rubber sound insulation pads and reduce the emission of volatile organic compounds and VOC gases.
[0167] Compared with Example 1, Comparative Example 4 uses a traditional sulfur vulcanization system and is not filled with a deodorizer. Its sound insulation pad product has a pungent sulfurized odor, and the odor level reaches Level 3; Comparative Example 5 uses a traditional sulfur vulcanization system, is not filled with a deodorizer, and is not filled with damping fillers such as mica powder, cork powder, and hollow glass beads. Its floor impact sound insulation improvement is only 22dB, and the odor level is as high as Level 4, which also proves the sound insulation effect of the damping filler.
[0168] Compared with Example 1, Comparative Example 1 is not filled with a deodorant, and its odor level is Level 2, which is higher than Level 0 of Example 1; Example 2 is not filled with layered mica powder, which is a damping filler, and its impact sound improvement is 29dB, which is lower than 35dB of Example 1. This is because the layered mica can effectively increase the number of reflections of sound waves in the sound insulation pad and accelerate the attenuation of the sound wave capacity; Comparative Example 2 is not filled with hollow glass microspheres, and its impact sound improvement is 28dB, which is lower than 35dB of Example 1, and its compression deformation is 15%, which is higher than 10% of the example. This is because the hollow glass microspheres can increase the rigidity of the sound insulation pad and ensure that it has better The compression rebound resilience of the hollow glass microspheres can form a better air isolation barrier to improve the sound insulation effect; Example 3 is not filled with rubber powder particles, and Comparative Example 3 is not filled with cork powder. The impact sound improvements are 31dB and 29dB, respectively, which are both lower than 35dB of Example 1. This is because the rubber powder particles and cork powder particles form a "sea-island" structure with the rubber at the microscopic level, and the microporous structure formed when the sound wave propagates through can effectively increase the loss of the sound wave; Example 4 is not filled with expanded graphite flame retardant, and its combustion performance grade is B2, which is lower than B1 in Example 1, and its safety is relatively low in actual use.
[0169] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A self-adhesive rubber sound insulation pad, characterized in that: The self-adhesive rubber sound insulation pad comprises: a vulcanized rubber sound insulation layer and a non-vulcanized butyl self-adhesive adhesive layer; The raw materials for preparing the vulcanized rubber sound insulation layer include: natural rubber, butyl rubber, a first filler, inorganic hollow microspheres, cork powder, a first activation processing aid, a first plasticizer, an odorless vulcanizing agent, an accelerator, an antioxidant, a deodorizing agent, optional rubber powder, an optional first flame retardant, an optional first tackifying resin, an optional anti-scorch agent and an optional release agent.
2. The self-adhesive rubber sound insulation pad according to claim 1, wherein: In parts by weight, relative to 100 parts of natural rubber, the butyl rubber is 10-50 parts, the rubber powder is 0-100 parts, the first filler is 150-350 parts, the first flame retardant is 0-50 parts, the inorganic hollow microspheres are 10-80 parts, the cork powder is 10-80 parts, the first activation processing aid is 3-10 parts, the first tackifying resin is 0-5 parts, the first plasticizer is 10-70 parts, the odorless vulcanizing agent is 1-5 parts, the accelerator is 1-3 parts, the scorch retarder is 0-2 parts, the antioxidant is 1-5 parts, the release agent is 0-4 parts, and the deodorizing agent is 5-20 parts.
3. The self-adhesive rubber sound insulation pad according to claim 1 or 2, wherein: The raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer include: butyl rubber, a second filler, a second activation processing aid, a second plasticizer, a second tackifying resin, an antioxidant, a light stabilizer, an optional second flame retardant and an optional polyisobutylene; Preferably, in parts by weight, relative to 100 parts of butyl rubber, the polyisobutylene is 0-50 parts, the second filler is 50-150 parts, the second flame retardant is 0-40 parts, the second activation processing aid is 1-10 parts, the second plasticizer is 2-30 parts, the second tackifying resin is 50-200 parts, the antioxidant is 1-3 parts, and the light stabilizer is 1-3 parts.
4. The self-adhesive rubber sound insulation pad according to claim 1 or 2, wherein: The first plasticizer is selected from at least one of naphthenic oil, paraffin oil, rosin oil and soybean oil; The first tackifying resin is selected from at least one of C5 petroleum resin, C9 petroleum resin and terpene resin; The first activation processing aid is selected from at least one of zinc oxide, stearic acid and zinc stearate; The first flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide, phosphorus nitrogen intumescent flame retardant and intumescent graphite flame retardant; The first filler is preferably selected from mica powder and an optional first other filler, and the first other filler is selected from at least one of carbon black, calcium carbonate, white carbon, clay and talc; further preferably, the mass ratio of the first other filler to the mica powder is (0-6):
1.
5. The self-adhesive rubber sound insulation pad according to claim 3, wherein: The second plasticizer is selected from at least one of naphthenic oil, paraffin oil, rosin oil and soybean oil; The second tackifying resin is selected from at least one of C5 petroleum resin, C9 petroleum resin and terpene resin; The second activation processing aid is selected from at least one of zinc oxide, stearic acid and zinc stearate; The second flame retardant is selected from at least one of aluminum hydroxide, magnesium hydroxide, phosphorus nitrogen intumescent flame retardant and intumescent graphite flame retardant; The second filler is preferably selected from mica powder and an optional second other filler, and the second other filler is selected from at least one of carbon black, calcium carbonate, white carbon, clay and talc; further preferably, the mass ratio of the second other filler to the mica powder is (0-6):
1.
6. The self-adhesive rubber sound insulation pad according to claim 1 or 2, wherein: The accelerator is selected from at least one of trimethallyl isocyanate, triallyl isocyanurate, N,N'-m-phenylene bismaleimide, trimethylolpropane methacrylate and p-benzoquinone dioxime; The scorch retarder is selected from at least one of N-cyclohexylthiophthalamide, phthalic anhydride and N-nitrosodiphenylamine; The antioxidant is at least one of antioxidant RD, antioxidant MB, antioxidant 4010NA and antioxidant 4020; The rubber powder is preferably selected from at least one of 20 mesh rubber powder, 50 mesh rubber powder and 100 mesh rubber powder; The odorless vulcanizing agent is preferably at least one selected from benzoyl hydroperoxide, diisopropyl di-tert-butyl peroxide and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.
7. The self-adhesive rubber sound insulation pad according to claim 1 or 2, wherein: The inorganic hollow microspheres are at least one of 40 mesh hollow glass microspheres, 80 mesh hollow glass microspheres, 120 mesh hollow glass microspheres, 40 mesh hollow ceramic microspheres, 80 mesh hollow ceramic microspheres and 120 mesh hollow ceramic microspheres; The cork powder is selected from at least one of 60-mesh cork powder, 100-mesh cork powder and 150-mesh cork powder.
8. The self-adhesive rubber sound insulation pad according to claim 3, wherein: The weight average molecular weight of the polyisobutylene is 1300-2400; The antioxidant is antioxidant 1010; The light stabilizer is BASF light stabilizer 2020.
9. The method for preparing the self-adhesive rubber sound insulation pad according to any one of claims 1 to 8, characterized in that: The preparation method comprises: (1) putting the natural rubber, butyl rubber and optional rubber powder into an internal mixer for internal mixing, then putting a first activated processing aid, an antioxidant, a deodorant, an optional first tackifying resin and an optional release agent into the internal mixer for internal mixing, and finally putting a first filler, inorganic hollow microspheres, cork powder, a first plasticizer and an optional first flame retardant into the internal mixer for internal mixing, and then removing the rubber; (2) placing the rubber material obtained in step (1) on an open mixing mill for mixing to obtain a mixed rubber; (3) putting the first-stage mixed rubber obtained in step (2) into an internal mixer for internal mixing, and then adding the odorless vulcanizing agent, accelerator and optional scorch retarder, and performing internal mixing and rubber removal; (4) placing the rubber material obtained in step (3) on an open mixing mill for mixing to obtain a two-stage mixed rubber; (5) the two-stage mixed rubber obtained in step (4) is made into a rubber coil in a screw extruder, and then the rubber coil is calendered and vulcanized at 160-170° C. on a drum vulcanizer to obtain the vulcanized rubber sound insulation layer; (6) mixing the raw materials for preparing the non-vulcanized butyl self-adhesive adhesive layer in an internal mixer to remove the adhesive; (7) Extrusion coating the self-adhesive rubber obtained in step (6) on the vulcanized rubber sound insulation layer to form a self-adhesive rubber layer, and then calendering it through a double-roll calender to obtain the self-adhesive rubber sound insulation pad.
10. Use of the self-adhesive rubber sound insulation pad according to any one of claims 1 to 8 as a vibration-damping sound insulation pad for building floating floors.
Citation Information
Cited By
Composition for sound absorption and noise reduction layer, raw material combination, waterproof coiled material and preparation method and application of waterproof coiled material
CN121105512A