Phosphorus-containing zinc ion battery negative electrode modifier, modification method and application thereof

By using nano-level SEI film modifiers in zinc ion batteries, the problem of zinc dendrites and hydrogen evolution reactions is solved, the cycle life and electrochemical performance of zinc ion batteries are improved, and the stable and efficient electrochemical performance of zinc ion batteries is achieved. .

CN119069706APending Publication Date: 2024-12-03BEIJING INST OF TECH

Patent Information

Application Number
CN202411199599.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The formation of zinc dendrites and hydrogen evolution reaction in zinc ion batteries leads to a reduced efficiency of the battery coulomb and a short cycle life. The existing modification strategies increase interfacial impedance while improving electrochemical performance while decreasing kinetics.

Method used

The organic phosphonic acid chelating agent composed of carbon atoms or nitrogen atoms connected to phosphonic acid groups is used as the zinc negative electrode modifier to generate a nano-scale dense SEI film, regulate the desolvation process of zinc, inhibit the hydrogen evolution reaction and the growth of zinc dendrites. .

Benefits of technology

The stable SEI film is formed to inhibit the hydrogen evolution reaction, regulate the uniform deposition of zinc, improve the cycle life and electrochemical performance of zinc ion batteries, improve the dynamic performance of the battery, and avoid battery short circuit and capacity decay.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069706A_ABST
    Figure CN119069706A_ABST
Patent Text Reader

Abstract

The invention relates to a phosphorus-containing zinc ion battery negative electrode modifier, a modification method and application thereof, and belongs to the technical field of zinc ion batteries. The anode modifier is one or more of 1-hydroxyethylidene-1, 1-diphosphonic acid, 1-hydroxyethylidene-1, 1-triphosphonic acid, amino trimethylene phosphonic acid, ethylenediamine tetramethylenephosphonic acid, diethylenetriamine pentamethylenephosphonic acid, bis (1, 6-hexylidene) triamine pentamethylenephosphonic acid and triethylene tetramine hexamethylenephosphonic acid; the zinc ion battery negative electrode modification method comprises the following steps: adding the modifier into water, uniformly mixing to obtain a mixed solution with the modifier concentration of 200-5000mg L <-1 >, the pH value of 3-7 and the temperature of 25-80 DEG C, then adding zinc foil, reacting for 1-30 minutes, and then taking out to obtain the zinc ion battery negative electrode. The modifier inhibits the reaction between zinc foil and active water molecules by adjusting a zinc ion solvation structure, improves nucleation overpotential, promotes deposition of zinc ions along a (002) crystal face, inhibits growth of zinc dendrites, and improves battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phosphorus-containing zinc ion battery negative electrode modifier, a modification method and application thereof, and belongs to the technical field of zinc ion batteries. Background Art

[0002] Energy is the foundation of the evolution of human civilization and the foundation of human production and life activities. The degree of energy development and utilization marks the degree of evolution and development of human society. Without large-scale and high-quality energy supply, human society cannot develop. From the perspective of the development of human history since modern times, every breakthrough in energy technology is accompanied by major changes in production technology, and even causes a revolution in social production methods. However, since the industrial revolution, environmental issues have increasingly become an obstacle to the development of human society; the consumption of non-renewable energy reserves has made the use of clean and green energy increasingly urgent. Especially since the first oil crisis in 1973, people have begun to realize that the modern industrial system based on oil is deeply constrained by international political factors and has its fragility. Against this background, the energy structure transition from oil and natural gas to new energy is quietly taking place. Among the many forms of energy, electrical energy is the most easily converted into various other forms of energy such as solar energy, wind energy, geothermal energy, and the various storage technologies of electrical energy are also the most convenient for electrochemical energy storage. The device that realizes the mutual conversion between chemical energy and electrical energy is called a chemical power source. Chemical power sources are less affected by factors such as terrain and can be flexibly used in the power generation side, power transmission and distribution side, and power consumption side. As a result, they have become the largest energy storage technology route in the field of large-scale energy storage besides pumped storage, and they play the most critical role in actual energy storage.

[0003] Since the first commercial lithium-ion battery system was launched in the 1990s, after 30 years of development, lithium-ion batteries have been developed on a large scale due to their high specific energy, good cycle performance and mature process routes. In most fields, they have gradually replaced the previously widely used secondary electrochemical systems such as nickel-hydrogen batteries. At present, lithium-ion batteries have been widely used in 3C mobile devices, power batteries and electrochemical energy storage. However, the abundance of lithium in the earth's crust is low (only about 20 mg kg -1 ), the mining cost is relatively high, the lithium, cobalt and other elements in lithium-ion batteries are strategic resources, and the balance of supply and demand is extremely fragile; at the same time, lithium-ion batteries are organic systems and involve the redox reaction of the relatively active lithium element, and their safety issues cannot be ignored, which hinders the larger-scale development of lithium-ion batteries.

[0004] In order to solve the problems encountered by lithium-ion batteries, researchers have developed secondary zinc-ion batteries as a new generation of electrochemical energy storage devices. Its system is somewhat different from traditional lithium-ion batteries. Its positive electrode is a zinc ion storage electrode, mainly manganese-based and vanadium-based materials; the negative electrode is metallic zinc. During the discharge and charging process of zinc-ion batteries, energy is stored and released through the reversible stripping / plating of zinc at the negative electrode and the insertion / deinsertion of zinc ions at the positive electrode, respectively. Compared with traditional lithium-ion battery systems, zinc-ion batteries have the following characteristics: (i) Low price. The abundance of zinc in the earth's crust is relatively high, about 94 mg / kg -1 , and its mining technology is mature, making its price much lower than lithium (about US$420 per ton, about 1 / 160 of lithium), which is conducive to large-scale deployment. (ii) Zinc has good compatibility with aqueous electrolytes. Zinc ions have a small hydration radius, which is conducive to ion embedding in typical layered structure positive electrode materials; at the same time, it is difficult to form a dense passivation film on the surface of zinc. If an organic electrolyte is used, it will greatly increase the internal resistance of the battery. For the above two reasons, zinc-ion batteries usually use aqueous electrolytes, so they are often called aqueous zinc-ion batteries (AZIBs). Thanks to the good compatibility of zinc with aqueous electrolytes, zinc-ion batteries have higher safety and ionic conductivity than lithium-ion batteries. (iii) Green and environmentally friendly. Aqueous electrolytes cause much less damage to nature than organic systems; at the same time, since zinc is a metal widely used in industry, its recycling technology is much more mature than lithium, causing less pollution. (iv) The redox reaction of zinc atoms is a two-electron reaction, and zinc has a high density, which makes it have a high volumetric capacity, about 3 times that of lithium metal. Such properties make Zn-ion batteries suitable for applications with high volumetric capacity requirements, such as large-scale energy storage systems (ESSs).

[0005] Zinc ions have extremely high theoretical specific capacity, low redox potential and low density. Therefore, zinc ion batteries using zinc ions as negative electrodes are considered to be one of the most promising high-energy storage devices with broad application prospects. However, the negative electrodes of zinc ion batteries have the following two main problems: (i) the formation of zinc dendrites. Similar to lithium metal batteries, during the electrochemical cycle, the deposition-stripping of zinc metal has intrinsic inhomogeneity, resulting in the appearance of micro-protrusions on the surface of metallic zinc. Due to the tip aggregation effect of electrons, the electric field on the surface of the micro-protrusions is stronger. In the subsequent electrochemical cycle, positively charged zinc ions tend to be adsorbed on the surface of more negatively charged micro-protrusions for deposition, thus forming zinc dendrites. The formation of zinc dendrites reduces the Coulombic efficiency of the battery. Since the Young's modulus of zinc is as high as 108GPa, which is much higher than that of lithium (5GPa) and sodium (10GPa), it is easy to pierce the diaphragm and short-circuit the battery. In addition, dendrites with poor adhesion to the metal substrate are easily separated from the zinc negative electrode, resulting in the generation of "dead zinc", thereby reducing the negative electrode capacity. (ii) Hydrogen evolution reaction (HER) occurs on the surface of metallic zinc. Due to the strong metallic activity of zinc (stronger than H), zinc metal will undergo hydrogen evolution reaction with the weakly acidic ZnSO4 electrolyte. The hydrogen and other gases produced by the hydrogen evolution reaction can cause a series of problems such as battery bloating and electrolyte leakage; at the same time, the hydrogen evolution reaction consumes water in the electrolyte, causing corrosion to the surface of the zinc negative electrode and reducing the amount of active zinc metal. The consumption of H in water leads to residual OH near the negative electrode-electrolyte interface. - Ions accumulate, and the pH value near the zinc negative electrode rises to 6-7.5; hydroxide ions and Zn 2+ Combined with other electrolyte components, it forms insulating byproducts such as zinc oxide, zinc hydroxide, and basic zinc sulfate, which are harmful to uniform zinc plating. The formation of these inactive substances and hydroxides will not only cause the Zn in the electrolyte to 2+ It not only reduces the irreversible loss of the zinc anode, but also reduces the Coulombic efficiency of the zinc negative electrode, thereby reducing the Coulombic efficiency of the entire zinc-ion battery.

[0006] Uniform zinc deposition and suppression of harmful hydrogen evolution side reactions are beneficial to improving the cycle stability and coulombic efficiency of zinc-ion batteries and extending their cycle life. In order to suppress the formation of zinc dendrites and the occurrence of HER, a series of strategies have been proposed, including electrolyte modification, diaphragm modification, main structure design, surface modification, etc. Among them, the surface modification of metallic zinc anode has attracted extensive attention from researchers because of its clear mechanism and easy control. However, a large number of surface modification strategies are to coat a micron-level modification layer on the surface of the zinc anode. While such a modification layer plays a role in suppressing the hydrogen evolution reaction and regulating the uniform deposition of zinc, it will inevitably bring about a large interfacial impedance, resulting in a decrease in the battery's kinetics and an increase in polarization. Summary of the invention

[0007] In view of this, in order to solve the problems of zinc dendrite growth and HER corrosion reaction in zinc ion batteries in the prior art, the purpose of the present invention is to provide a phosphorus-containing zinc ion battery negative electrode modifier, modification method and application thereof. The zinc negative electrode modified by the present invention can generate a layer of nano-scale dense SEI film on the surface of zinc foil, and its strong chelating ability with zinc helps to regulate the desolvation process of zinc, and the intrinsic hydrophobic property can inhibit the occurrence of hydrogen evolution reaction. At the same time, the nano-scale modification layer does not increase the ionic conductivity of the SEI film. On the whole, the zinc negative electrode based on the modifier can form a stable SEI film, inhibit the occurrence of hydrogen evolution reaction, and regulate the uniform deposition of zinc, which not only inhibits the growth of zinc dendrites, improves the cycle life of zinc ion batteries, but also improves the electrochemical performance of the whole battery. The SEI film and zinc electrode can both inhibit the growth of zinc dendrites and make the battery have good electrochemical performance.

[0008] To achieve the purpose of the present invention, the following technical solutions are provided.

[0009] A phosphorus-containing zinc ion battery negative electrode modifier, wherein the negative electrode modifier is a phosphonic acid group connected by a carbon atom or a nitrogen atom Composition of organic phosphonic acid chelating agent.

[0010] Preferably, the total number of carbon atoms or nitrogen atoms connected to the phosphonic acid group is 1-3.

[0011] Preferably, the total number of all phosphonic acid groups connected to the carbon atom or nitrogen atom is 2-6.

[0012] More preferably, the organic phosphonic acid chelating agent is one or more of hydroxyethylidene diphosphonic acid, hydroxyethylidene triphosphonic acid, aminotrimethylene phosphonic acid, ethylenediaminetetramethylene phosphonic acid, diethylenetriaminepentamethylene phosphonic acid, bis(1,6-hexylene)triaminepentamethylene phosphonic acid, and triethylenetetraaminehexamethylene phosphonic acid.

[0013] A method for modifying a negative electrode of a zinc ion battery, the method comprising the following steps:

[0014] (1) adding the modifier of claim 1 to water, mixing uniformly to obtain a mixed solution, adjusting the pH of the solution, and then continuously heating the solution;

[0015] (2) Add the pre-cleaned zinc foil to the solution described in (1), take it out after a period of reaction, and wash it with distilled water and anhydrous ethanol and dry it.

[0016] Preferably, in step (1), the total concentration of the modifier in the mixed solution is 200 mg L -1 ~5000mgL -1, the heating temperature is 25 to 80° C., and the pH value is adjusted to 3 to 7; in step (2), the zinc foil is immersed in the electrolyte modifier for chemical modification for a modification time of 1 to 30 minutes.

[0017] More preferably, in step (1), the total concentration of the modifier in the mixed solution is 500 mg L -1 , the heating temperature is 60° C., and the pH value is adjusted to 6-7; in step (2), the zinc foil is immersed in the electrolyte modifier for chemical modification for 15 minutes.

[0018] An application of the phosphorus-containing zinc ion battery negative electrode modifier of the present invention comprises: adding pre-cleaned zinc foil to 200 mg L -1 ~5000mg L -1 The solution of the present invention with a concentration of 100 μg / cm2 is reacted at 25 to 80° C. for 1 to 30 min, then taken out, washed with distilled water and anhydrous ethanol, and dried.

[0019] A zinc negative electrode with an artificial SEI film is a zinc negative electrode prepared by applying the phosphorus-containing modifier of the present invention.

[0020] A zinc ion battery, wherein the negative electrode of the battery is a zinc negative electrode with an artificial SEI film prepared by applying the modifier of the invention.

[0021] Beneficial Effects

[0022] (1) The present invention provides a phosphorus-containing zinc ion battery negative electrode modifier, wherein the phosphonic acid group fragment of the modifier is compatible with the zinc ion battery electrolyte system, and the organic molecule has good biocompatibility and is non-toxic and harmless; during the modification process, a nano-scale dense SEI film can be generated on the surface of the zinc foil, and its strong chelating ability with zinc helps to regulate the desolvation process of zinc in the electrochemical cycle, and its intrinsic hydrophobic property can prevent the direct contact between the water molecules coordinated with the zinc ions and the zinc negative electrode, thereby inhibiting the occurrence of hydrogen evolution reaction. The zinc negative electrode based on the modifier can form a stable SEI film, inhibit the occurrence of hydrogen evolution reaction, and regulate the uniform deposition of zinc, which not only inhibits the growth of zinc dendrites, improves the cycle life of the zinc ion battery, but also improves the electrochemical performance of the battery.

[0023] (2) The present invention provides a method for modifying the negative electrode of a zinc ion battery, which is simple and easy to implement. Since the method for modifying the negative electrode of a zinc ion battery contains the negative electrode modifier of the present invention, the method can be used to modify the zinc negative electrode, thereby inhibiting the occurrence of corrosion reactions and improving the cycle life and working performance of the zinc ion battery. In the application of electrodes or batteries, the artificial SEI film formed can be made uniform and dense, thereby enabling the battery to have a stable long-term cycle and good electrochemical performance.

[0024] (3) The present invention provides an application of a phosphorus-containing negative electrode modifier for zinc ion batteries. The chemical modification method used in the application is simple and easy, and the thickness is adjustable, so it is easy to obtain a flat and dense zinc negative electrode modification layer. At the same time, the low thickness of the modification layer can avoid the problem of poor reaction kinetics caused by a thick modification layer applied by scraping, brushing, etc.

[0025] (4) The present invention provides a zinc negative electrode with an artificial SEI film, wherein the surface of the zinc negative electrode has a uniform and dense artificial SEI film generated by chelating zinc with an organic phosphonic acid, and the film-forming conditions have a certain degree of controllability; and the application is that before the electrochemical cycle, the zinc electrode body is pre-reacted with the modifier described in the present invention, that is, the SEI film is prefabricated on the surface of the zinc electrode body in advance, to obtain a zinc ion electrode with a SEI film, and then the electrode is applied to a zinc ion battery, thereby reducing the consumption of additive molecules during the cycle and being more conducive to the regulation of desolvation.

[0026] (5) The present invention provides a zinc ion battery, wherein the zinc negative electrode of the battery has relatively uniform zinc ion deposition during the cycle, and the growth of zinc dendrites is suppressed, thereby improving the cycle performance of the battery and stably performing the electrochemical performance of the battery at a high level; the assembled zinc-zinc symmetric battery has a small polarization, and a safe and long-lasting zinc ion battery can be obtained, which is beneficial to stably improving the cycle life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The Zn||Zn symmetric battery assembled from the control group zinc foil in Test Example 1 at 5 mA cm -2 , 1mAh cm -2 The following is the cycle test result diagram.

[0028] Figure 2 The Zn||Zn symmetric battery assembled from the zinc foil of the experimental group in Test Example 1 is 5 mA cm -2 , 1mAh cm -2 The following is the cycle test result diagram.

[0029] Figure 3The Zn||LiMn2O4 full battery assembled from the experimental group and the control group zinc foil in test example 1 was tested at 2C (1C = 148 mAh g -1 ) under the cycle test results. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels or prepared according to literature unless otherwise specified.

[0031] Example 1

[0032] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0033] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 A HEDP solution of 1.5% concentration was prepared. With a magnetic stirrer at a speed of 700 rpm, 5% by mass of dilute ammonia water was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Stirring was continued to ensure that the solution was evenly mixed, and the magnetic stirrer was set to 60°C to heat the mixed solution until the solution temperature was maintained at 60°C.

[0034] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0035] Example 2

[0036] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0037] (1) Dilute the aminotri(methylenephosphonic acid) (ATMP) solid or concentrated solution with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1ATMP solution of 1.5% concentration. Add 5% by mass of dilute ammonia water dropwise to the ATMP solution at a magnetic stirrer speed of 700 rpm, and use a pH meter to measure the pH value of the ATMP solution until the pH value of the solution is adjusted to 6.5. Continue stirring to ensure that the solution is evenly mixed, and set the magnetic stirrer to 60°C to heat the mixed solution until the solution temperature is maintained at 60°C.

[0038] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0039] Example 3

[0040] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0041] (1) Dilute ethylenediaminetetraethylenephosphonic acid (EDTMP) solid or concentrated solution with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 Concentration of EDTMP solution. At a magnetic stirrer speed of 700 rpm, 5% mass fraction of dilute ammonia water was added dropwise to the EDTMP solution, and the pH value of the EDTMP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Continue stirring to ensure that the solution is evenly mixed, and at the same time, set the magnetic stirrer to 60°C and heat the mixed solution until the solution temperature is maintained at 60°C.

[0042] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0043] Example 4

[0044] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0045] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 1000 mg L -1 A HEDP solution of 1.5% concentration was prepared. With a magnetic stirrer at a speed of 700 rpm, 5% by mass of dilute ammonia water was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Stirring was continued to ensure that the solution was evenly mixed, and the magnetic stirrer was set to 60°C to heat the mixed solution until the solution temperature was maintained at 60°C.

[0046] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0047] Example 5

[0048] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0049] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 Concentration of HEDP solution. At a magnetic stirrer speed of 700 rpm, 5% mass fraction of dilute ammonia water was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 3. Continue stirring to ensure that the solution is evenly mixed, and at the same time, set the magnetic stirrer to 60°C to heat the mixed solution until the solution temperature is maintained at 60°C.

[0050] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0051] Example 6

[0052] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0053] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 A HEDP solution of 1.5% concentration was prepared. With a magnetic stirrer at a speed of 700 rpm, 5% by mass of dilute ammonia water was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Stirring was continued to ensure that the solution was evenly mixed, and the magnetic stirrer was set to 60°C to heat the mixed solution until the solution temperature was maintained at 60°C.

[0054] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 10 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0055] Example 7

[0056] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0057] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 Concentration of HEDP solution. Under a magnetic stirrer at a speed of 700 rpm, 5% mass fraction of dilute ammonia water was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Stirring was continued at room temperature of 25°C for 1 hour to ensure that the solution was evenly mixed.

[0058] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. At room temperature of 25°C and a rotation speed of 200 rpm, the zinc foil is immersed in the modification solution obtained in (1), reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0059] Example 8

[0060] A zinc ion battery negative electrode, the preparation method of which is as follows:

[0061] (1) Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 Concentration of HEDP solution. At a magnetic stirrer speed of 700 rpm, 5% mass fraction of KOH solution was added dropwise to the HEDP solution, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. Stirring was continued to ensure that the solution was evenly mixed, and the magnetic stirrer was set to 60°C to heat the mixed solution until the solution temperature was maintained at 60°C.

[0062] (2) The zinc foil is cut into appropriate specifications, cleaned with detergent, deionized water, and anhydrous ethanol in sequence, and placed in 5 mM dilute hydrochloric acid for 1 minute of ultrasonic treatment to remove the oxide layer on the surface, and then the hydrochloric acid remaining on the surface is cleaned with deionized water and anhydrous ethanol, and dried for use. The zinc foil is immersed in the modification solution obtained in (1) at a rotation speed of 200 rpm, reacted for 15 minutes, and then taken out, and the modification solution remaining on the surface is cleaned with deionized water and anhydrous ethanol, and then dried with cold air to obtain a zinc ion battery negative electrode with an artificial SEI film.

[0063] Example 9

[0064] A zinc ion battery negative electrode modifier, the preparation method of which is as follows:

[0065] Dilute the solid or concentrated solution of hydroxyethylidene diphosphonic acid (HEDP) with deionized water and stir evenly with a magnetic stirrer to mix thoroughly to prepare 500 mg L -1 A HEDP solution of 1.5% concentration was prepared. A 5% by mass fraction of dilute ammonia water was added dropwise to the HEDP solution at a magnetic stirrer speed of 700 rpm, and the pH value of the HEDP solution was measured using a pH meter until the pH value of the solution was adjusted to 6.5. The stirring was continued for 1 hour to ensure that the solution was evenly mixed, thereby obtaining a negative electrode modifier for zinc ion batteries.

[0066] Test Example 1

[0067] The zinc foil prepared in Example 1 was assembled into a button symmetrical battery with a glass fiber separator and a 2M ZnSO4 electrolyte (referred to as the experimental group);

[0068] Bare zinc foil, glass fiber separator and 2M ZnSO4 electrolyte were used to assemble button symmetrical cells (referred to as the control group);

[0069] The assembly order of the button symmetrical batteries in the experimental group and the control group is: positive electrode shell, zinc sheet, 150 μL electrolyte, diaphragm, zinc sheet, stainless steel gasket, stainless steel spring and negative electrode shell; after assembly, the battery is pressed using a punch. -2 , with a capacity of 1 mAh cm -2 The charge and discharge test was carried out under the following conditions, and the test results were as follows Figure 1 and Figure 2 shown.

[0070] It can be seen that the curve overpotential of the experimental group Zn||Zn symmetric battery is low (only ~36mV after stable cycling), providing a stable cycle of more than 2000h; while the overpotential of the control group Zn||Zn symmetric battery is ~65mV, and as the cycle progresses, the overpotential increases significantly. Finally, at ~160h of cycling, the overpotential of the battery increases sharply, indicating that the corrosion byproduct of the battery during the cycle, basic zinc sulfate, covers the surface of the zinc foil. The insulating basic zinc sulfate increases the polarization of the battery during the electrochemical cycle, causing the battery to short-circuit and interrupt the cycle. 5mA cm -2 、1mAh cm -2 The stable operation of the zinc symmetric battery under these conditions indicates that the battery assembled with the modified zinc negative electrode still has very good kinetic performance under high current density. The protective film formed on the surface of the zinc negative electrode can prevent the formation of dendrites, while inhibiting the occurrence of hydrogen evolution reaction and preventing battery short circuit.

[0071] Test Example 2

[0072] The zinc foil prepared in Example 1 was assembled into a button full battery (referred to as the experimental group) with a glass fiber separator, a 2M ZnSO4+1M Li2SO4 electrolyte, and a LiMn2O4 positive electrode.

[0073] The button cells were assembled with bare zinc foil and glass fiber separator, 2M ZnSO4+1M Li2SO4 electrolyte, and LiMn2O4 positive electrode (referred to as the control group);

[0074] The LiMn2O4 positive electrode plate is a plate obtained by coating and drying commercially available LiMn2O4 material: polyvinylidene fluoride: conductive carbon black in a ratio of 8:1:1 and then cutting.

[0075] The assembly order of the button cells in the experimental and control groups is: positive electrode shell, LiMn2O4 positive electrode sheet, 150μL electrolyte, diaphragm, zinc sheet, stainless steel gasket, stainless steel spring and negative electrode shell; after assembly, the battery is pressed using a punch. -1 ) to carry out charge and discharge test, and the test results are as follows Figure 3 shown.

[0076] Depend on Figure 3 It can be seen that the capacity of the full battery in the control group declined severely after 125 cycles. This is because the formation of zinc dendrites made it difficult to further exert the electrochemical potential of the zinc negative electrode. The full battery assembled in the experimental group achieved 250 cycles and still maintained 55 mAh g -1 The cycling performance of the full battery and the stable long cycle of the symmetric battery together show that the modified zinc anode has great potential in inhibiting dendrite growth, maintaining high specific capacity and coulombic efficiency of the battery, and extending the service life of the battery.

[0077] In addition, various characterization tests such as scanning electron microscopy, in-situ optical microscopy, and in-situ differential electrochemical mass spectrometry were carried out. The results of various characterization tests all support the good effect of organic phosphonic acid chelating agents on the modification of zinc negative electrodes. The zinc deposited on the modified negative electrode is smooth and dense, without obvious dendrite growth, corresponding to the deposition parallel to the (002) crystal plane. Its deposition is uniform and the deposition performance is good, which is conducive to the long cycle performance of the battery. Under the same current density and deposition capacity, there is obvious dendrite growth perpendicular and oblique to the zinc substrate on the unmodified negative electrode, showing that the dominant crystal planes of its growth are (100) and (101) crystal planes. Zinc metal has a high Young's modulus, and the growth mode that is not parallel to the surface of the zinc foil substrate can easily cause dendrites to pierce the diaphragm and cause a short circuit in the battery. In contrast, the deposition of zinc on the modified negative electrode still tends to be smooth and dense, which is conducive to long and stable battery cycles. In the application of electrodes or batteries, the formed artificial SEI film can be made uniform and dense, so that the battery can have a stable long-term cycle, avoid the capacity decay of the zinc ion battery, and show excellent electrochemical performance.

[0078] The zinc negative electrodes provided in other embodiments were tested with reference to the above method. Compared with the unmodified electrolyte or electrode, the negative electrodes showed an inhibitory effect on the hydrogen evolution reaction, a flatter overpotential and better cycle stability, and improved coulombic efficiency. This further illustrates the effect of the negative electrode modifier provided by the organic phosphonic acid chelating agent proposed in the present invention on improving the battery cycle performance, and the significant effect of inhibiting the dendrite growth and hydrogen evolution reaction of zinc ion batteries.

[0079] The present invention includes but is not limited to the above embodiments. Any equivalent replacement or partial improvement made under the principle of the spirit of the present invention shall be deemed to be within the protection scope of the present invention.

Claims

1. A phosphorus-containing zinc ion battery negative electrode modifier, characterized in that: The negative electrode modifier is an organic phosphonic acid chelating agent composed of a central carbon atom or a nitrogen atom connected to a phosphonic acid group; the organic phosphonic acid chelating agent is one or more of hydroxyethylidene diphosphonic acid, hydroxyethylidene triphosphonic acid, aminotrimethylene phosphonic acid, ethylenediaminetetramethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, bis(1,6-hexylene)triaminepentamethylenephosphonic acid, and triethylenetetraaminehexamethylenephosphonic acid.

2. A method for modifying a negative electrode of a zinc ion battery as claimed in claim 1, characterized in that: The method steps are as follows: (1) adding one or more modifiers in claim 1 to water, mixing uniformly to obtain a mixed solution, and adjusting the pH of the solution to 6 to 7; (2) Add the pre-cleaned zinc foil to the solution described in (1), take it out after a period of reaction, and wash it with distilled water and anhydrous ethanol and dry it.

3. a method for modifying a zinc ion battery negative pole according to claim 2, characterized in that: The total concentration of the modifiers is 200 mg L -1 ~5000mg L -1 .

4. A method for modifying a negative electrode of a zinc ion battery according to claim 2 to 3, characterized in that: The zinc foil is immersed in the electrolyte modifier for chemical modification for 1 to 30 minutes.

5. A method for modifying a negative electrode of a zinc ion battery according to claims 2 to 4, characterized in that: The modification temperature of the zinc foil being immersed in the electrolyte modifier for chemical modification is 25-80°C.

6. An application of a zinc ion battery modifier as claimed in any one of claims 2 to 5, characterized in that: Pre-cleaned zinc foil was added to 200 mg L -1 ~5000mg L -1 The solution of claim 1 with a concentration of 200 μg / cm2 is reacted at 25 to 80° C. for 1 to 30 min, then taken out, washed with distilled water and anhydrous ethanol, and dried.

7. A zinc negative electrode having an artificial SEI film, characterized in that: The zinc negative electrode is a zinc negative electrode prepared by using the modifier described in claim 1, or a zinc negative electrode prepared by using the modification method described in any one of claims 2 to 5, or a zinc negative electrode prepared by using the modifier described in claim 6.

8. A zinc ion battery, characterized in that: The negative electrode of the battery is the zinc negative electrode with SEI film as claimed in claim 7.

Citation Information

Patent Citations

  • Electrolyte additive, electrolyte containing additive and lithium metal battery

    CN112103562A

  • Organic zinc phosphate-silane composite passive film modified zinc metal negative electrode and preparation method and application thereof

    CN113690401A

  • Electrolyte for zinc secondary battery and preparation method thereof

    CN115472923A

  • Method for in-situ generation of protective film on surface of metal anode of zinc ion battery and application thereof

    CN115528319A

  • Large-scale zinc negative electrode protection layer in-situ construction method, zinc negative electrode and application of zinc negative electrode

    CN116864601A

Cited By

  • Preparation method of modified zinc negative electrode, modified zinc negative electrode and aqueous zinc ion battery

    CN121149249A

  • Preparation method of modified zinc negative electrode, modified zinc negative electrode and aqueous zinc ion battery

    CN121149249B

  • Aqueous zinc ion battery electrolyte, preparation method thereof and zinc ion battery

    CN121260957A