Secondary battery, preparation method thereof, isolating membrane and electric device
By setting an initiator in the inorganic layer of the porous base film to form a gel electrolyte, the problem of insufficient conductivity of the gel electrolyte is solved, the power performance and production efficiency of the secondary battery are improved, and the energy density is achieved. Lower cost.
Patent Information
- Application Number
- CN202310638068.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The low ionic conductivity of gel electrolytes leads to low power performance of secondary batteries. How to improve the power performance of secondary batteries is an urgent problem.
By providing an initiator in the inorganic layer of the porous base film, a gel electrolyte is formed, the mechanical strength and ion transport capability of the isolation film are improved, and initiators are reduced or eliminated in the electrolyte raw material, thereby promoting rapid infiltration of the electrolyte and Cured to form a gel electrolyte in the inorganic layer.
It improves the power performance and production efficiency of the secondary battery, reduces costs, and improves the infiltration efficiency of the electrolyte and the energy density of the battery.
Smart Images

Figure CN119069784A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a secondary battery and a preparation method thereof, an isolation membrane and an electrical device. Background Art
[0002] Secondary batteries are widely used in various consumer electronic products and electric vehicles due to their outstanding features such as light weight, no pollution, and no memory effect. The electrolytes in secondary batteries include liquid electrolytes, gel electrolytes, and all-solid electrolytes according to their state.
[0003] Compared with liquid electrolytes, gel electrolytes have the advantages of higher safety and stability. However, due to the limitation of ionic conductivity of gel electrolytes, their disadvantage is that the power performance of batteries is low. Therefore, how to improve the power performance of such secondary batteries is an urgent problem to be solved. Summary of the invention
[0004] Based on this, it is necessary to provide a secondary battery and a preparation method thereof, a separator and an electrical device, which can improve the power performance of the secondary battery.
[0005] In a first aspect of the present application, a secondary battery is provided, comprising:
[0006] Positive electrode;
[0007] A negative electrode sheet, arranged opposite to the positive electrode sheet;
[0008] A separator, disposed between the positive electrode plate and the negative electrode plate, the separator comprising a porous base film and an inorganic layer, the components of the inorganic layer comprising inorganic particles and an initiator, and the inorganic layer being disposed on at least one surface of the porous base film; and
[0009] The gel electrolyte is disposed between the positive electrode plate and the separator, between the negative electrode plate and the separator, and in the inorganic layer of the separator. The initiator can initiate a polymerization reaction to form the gel electrolyte.
[0010] Without wishing to be limited to any theory, compared to directly setting the initiator in the pores or surface of the porous base membrane, the isolation membrane used in the above-mentioned secondary battery of the present application sets the initiator in the inorganic layer on the surface of the porous base membrane, and the initiator can initiate the polymerization of the polymerized monomers in the electrolyte to form a gel electrolyte. On the one hand, the presence of the inorganic layer can improve the mechanical strength of the isolation membrane. On the other hand, setting the initiator in the inorganic layer can make it unnecessary to add the initiator to the electrolyte raw material, thereby reducing the viscosity of the electrolyte raw material during injection, and enabling the electrolyte raw material to be quickly and fully infiltrated in the battery cell. The initiator in the inorganic layer of the isolation membrane dissolves after contacting the electrolyte raw material and enters the fully infiltrated electrolyte, and then solidifies under heating conditions, so that a gel electrolyte is formed inside the inorganic layer of the isolation membrane and between the isolation membrane and the positive electrode and / or the negative electrode. In particular, the gel electrolyte in the inorganic layer can not only improve the flexibility of the inorganic layer and its adhesion to the porous base membrane, but also improve its ability to transmit ions, thereby improving the power performance of the secondary battery. In addition, thanks to the improved efficiency of electrolyte raw material infiltration, the production cycle of the secondary battery is shortened, which is conducive to reducing costs.
[0011] In any embodiment of the present application, the initiator includes a free radical polymerization initiator;
[0012] Optionally, the free radical polymerization initiator includes at least one of an anionic and cationic initiator and an organic peroxide initiator;
[0013] More optionally, the anionic and cationic initiator includes at least one of a persulfate initiator and lithium acetate; more optionally, the organic peroxide initiator includes at least one of benzoyl peroxide, tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide.
[0014] In any embodiment of the present application, the initiator comprises lithium acetate.
[0015] In any embodiment of the present application, the inorganic particles include at least one of Al oxide, Al nitride, Al fluoride, Si oxide, Si nitride, Si fluoride, Fe oxide, Fe nitride, Fe fluoride, Fe oxyacid, Ti oxide, Ti nitride, Ti fluoride, Co oxide, Co nitride, Co fluoride, Ni oxide, Ni nitride, Ni fluoride, Mn oxide, Mn nitride, Mn fluoride, Sn oxide, Sn nitride, Sn fluoride, ZnO, barium titanate and lithium aluminum titanium phosphate;
[0016] Optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, SiO, SnO2, ZnO, Fe2O3, NiO, CuO, FePO4, barium titanate and lithium aluminum titanium phosphate;
[0017] More optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, barium titanate and lithium aluminum titanium phosphate.
[0018] In any embodiment of the present application, at least one of the following conditions is met:
[0019] (1a) The Dv50 particle size of the inorganic particles is 50 nm to 70 nm;
[0020] (1b) The thickness of the inorganic layer is 1 μm to 4 μm, and can be 2 μm to 4 μm.
[0021] In any embodiment of the present application, at least one of the following conditions is met:
[0022] (2a) The thickness of the porous base film is 4 μm to 20 μm, and can be 7 μm to 12 μm;
[0023] (2b) The average pore size of the porous base membrane is ≤200 nm, and can be selected from 10 nm to 200 nm;
[0024] (2c) The porosity of the porous base film is 30% to 80%;
[0025] (2d) The material of the porous base film includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, glass fiber, non-woven fabric and natural fiber.
[0026] In any embodiment of the present application, the gel electrolyte comprises an electrolyte salt and a polymer;
[0027] Optionally, the polymerization monomer of the polymer includes at least one of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, butyl acrylate, n-octyl methacrylate, n-octyl acrylate, vinyl acetate, vinylene carbonate, acrylonitrile, vinyl ethylene carbonate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, allyl methacrylate, divinylbenzene, polyvinyl alcohol, hexafluoropropylene, trichloroethylene, tetrafluoroethylene, chlorotrifluoroethylene and styrene.
[0028] In any embodiment of the present application, the secondary battery further comprises a liquid electrolyte, and the mass content of the gel electrolyte to the sum of the mass of the gel electrolyte and the liquid electrolyte is 60% to 100%, optionally 60% to 90%, and more optionally 60% to 80%.
[0029] In a second aspect of the present application, a method for preparing a secondary battery is provided, comprising the following steps:
[0030] forming an inorganic layer on at least one surface of the porous base film, wherein the components of the inorganic layer include inorganic particles and an initiator, to obtain a separator;
[0031] The negative electrode sheet, the separator and the positive electrode sheet are stacked and assembled to obtain a battery cell;
[0032] Electrolyte raw materials are injected into the battery core and heated for in-situ curing, so that the initiator triggers at least a portion of the electrolyte raw materials to polymerize in-situ and form a gel electrolyte; the components of the electrolyte raw materials include electrolyte salt, polymerization monomers and solvent.
[0033] In any embodiment of the present application, at least one of the following conditions is met:
[0034] (3a) the electrolyte salt comprises at least one of a sodium salt, a lithium salt and a potassium salt;
[0035] (3b) The solvent includes at least one of an ether solvent, an ester solvent and a sulfone solvent.
[0036] In a third aspect of the present application, an isolation film is provided, comprising:
[0037] A porous base membrane; and
[0038] The inorganic layer comprises inorganic particles and an initiator, and the inorganic layer is arranged on at least one surface of the porous base film.
[0039] In any embodiment of the present application, the mass content of the initiator in the inorganic layer is 1% to 10%, optionally 1% to 6%, and more optionally 1% to 3%.
[0040] In a fourth aspect of the present application, an electrical device is provided, wherein the electrical device comprises the secondary battery of the first aspect of the present application or the secondary battery prepared by the preparation method of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0042] Figure 1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0043] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown;
[0044] Figure 3 is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source;
[0045] Description of reference numerals:
[0046] 1. Secondary battery; 11. Casing; 12. Electrode assembly; 13. Cover plate; 2. Electrical device. DETAILED DESCRIPTION
[0047] Hereinafter, the embodiments of the secondary battery, preparation method and electric device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0048] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0051] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0052] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0053] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0054] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0055] The "filling coefficient" refers to the ratio of the amount of electrolyte injected to the cell capacity. Its unit can be g / Ah. Its physical meaning is the amount of electrolyte required to obtain the same capacity of the cell. Generally speaking, the smaller the filling coefficient, the smaller the overall mass of the battery and the higher the energy density.
[0056] Secondary battery
[0057] A secondary battery is a battery that can be recharged to activate the active materials after being discharged and continue to be used.
[0058] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, and an electrolyte. The electrolyte is disposed between the positive electrode sheet and the negative electrode sheet, and plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. During the battery charging and discharging process, the active ions in the active material are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet.
[0059] In some embodiments, the secondary battery further includes a separator, which is disposed between the positive electrode sheet and the negative electrode sheet to perform a separation function.
[0060] On one hand, the present application provides an isolation membrane, including a porous base membrane and an inorganic layer. The components of the inorganic layer include inorganic particles and an initiator. The inorganic layer is provided on at least one surface of the porous base membrane. The initiator can initiate polymerization of polymerizable monomers in the electrolyte to form a gel electrolyte; that is, the initiator can initiate a polymerization reaction to form a gel electrolyte. Specifically, a gel electrolyte is formed between the positive electrode plate and the isolation membrane, between the negative electrode plate and the isolation membrane, and in the inorganic layer of the isolation membrane.
[0061] Without wishing to be limited to any theory, compared to directly setting the initiator in the pores or surface of the porous base membrane, the isolation membrane used in the above-mentioned secondary battery of the present application sets the initiator in the inorganic layer on the surface of the porous base membrane, and the initiator can initiate the polymerization of the polymerized monomers in the electrolyte to form a gel electrolyte. On the one hand, the presence of the inorganic layer can improve the mechanical strength of the isolation membrane. On the other hand, setting the initiator in the inorganic layer can make it unnecessary to add the initiator to the electrolyte raw material, thereby reducing the viscosity of the electrolyte raw material during injection, and enabling the electrolyte raw material to be quickly and fully infiltrated in the battery cell. The initiator in the inorganic layer of the isolation membrane dissolves after contacting the electrolyte raw material and enters the fully infiltrated electrolyte, and then solidifies under heating conditions, so that a gel electrolyte is formed inside the inorganic layer of the isolation membrane and between the isolation membrane and the positive electrode and / or the negative electrode. In particular, the gel electrolyte in the inorganic layer can not only improve the flexibility of the inorganic layer and its adhesion to the porous base membrane, but also improve its ability to transmit ions, thereby improving the power performance of the secondary battery. In addition, thanks to the improved efficiency of electrolyte raw material infiltration, the production cycle of the secondary battery is shortened, which is conducive to reducing costs.
[0062] The porous base membrane can be any known porous structure film with good chemical stability and mechanical stability. In some embodiments, the material of the porous base membrane includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, glass fiber, non-woven fabric and natural fiber.
[0063] It is understood that the inorganic layer can be provided on one surface or two opposite surfaces of the porous base membrane. It is understood that in another embodiment, both surfaces of the porous base membrane are provided with inorganic layers, one of which contains an initiator and the other does not contain an initiator. The inorganic layer is combined with the porous base membrane to improve the mechanical strength of the separator.
[0064] In some embodiments, the initiator includes a free radical polymerization initiator. Further, the free radical polymerization initiator includes at least one of an anionic and cationic initiator and an organic peroxide initiator.
[0065] Optionally, the anionic and cationic initiator includes at least one of a persulfate initiator and lithium acetate, wherein the persulfate initiator includes but is not limited to potassium persulfate.
[0066] Optionally, the organic peroxide initiator includes at least one of benzoyl peroxide (BPO), tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide.
[0067] Further, the initiator includes lithium acetate.
[0068] In some embodiments, the inorganic particles include at least one of Al oxide, Al nitride, Al fluoride, Si oxide, Si nitride, Si fluoride, Fe oxide, Fe nitride, Fe fluoride, Fe oxyacid, Ti oxide, Ti nitride, Ti fluoride, Co oxide, Co nitride, Co fluoride, Ni oxide, Ni nitride, Ni fluoride, Mn oxide, Mn nitride, Mn fluoride, Sn oxide, Sn nitride, Sn fluoride, ZnO, barium titanate and lithium aluminum titanium phosphate. These inorganic particles can undergo redox reactions with materials including sodium metal and lithium metal, so that the inorganic particles can undergo redox reactions with lithium dendrites or sodium dendrites, which is beneficial to improving the efficiency of eliminating lithium dendrites or sodium dendrites, thereby further improving the power performance of the secondary battery.
[0069] Optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, SiO, SnO2, ZnO, Fe2O3, NiO, CuO, FePO4, barium titanate and lithium aluminum titanium phosphate; more optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, barium titanate and lithium aluminum titanium phosphate.
[0070] In some embodiments, the Dv50 particle size of the inorganic particles is 50 nm to 70 nm. The volume average particle size Dv50 of the inorganic particles is well known in the art and can be tested by methods known in the art. For example, it can be measured using a laser particle size analyzer (such as Malvern Master Size 3000). Wherein, Dv50 represents the particle size corresponding to when the cumulative volume distribution percentage of the inorganic particles reaches 50%.
[0071] In some embodiments, the thickness of the inorganic layer is 1 μm to 4 μm, such as 1 μm, 2 μm, 3 μm, 4 μm, and optionally 2 μm to 4 μm, 2 μm to 3 μm.
[0072] In some of the embodiments, the thickness of the porous base membrane is 4 μm to 20 μm, and optionally 7 μm to 12 μm.
[0073] In some embodiments, the average pore size of the porous base film is ≤200nm, and can be selected from 10nm to 200nm. The average pore size is a well-known meaning in the art and can be tested by methods known in the art. In addition, the average pore size is determined by the following method: the surface of the material is magnified by a microscope photograph, the number of pores per inch (25.4mm) is calculated as the number of cells, and then the average pore size is calculated by the following equation: average pore size = 25.4mm / number of cells.
[0074] In some embodiments, the porosity of the porous base film is 30% to 80%. The porosity is defined by the following equation: Porosity = (1-(mass of porous material [g] / (volume of porous material [cm3]×material density)))×100[%]. The porosity of the membrane layer can be measured by the mercury intrusion method and gas adsorption method according to GB / T 21650.2-2008.
[0075] The following will introduce in detail the preparation method of the isolation membrane and the preparation method of the secondary battery.
[0076] It can be understood that the above-mentioned separator can be prepared by forming an inorganic layer on at least one surface of a porous base film.
[0077] In some embodiments, in the isolation film, the mass content of the initiator in the inorganic layer is 1% to 10%. As an example, the content of the initiator in the inorganic layer is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, optionally 1% to 6%, and more optionally 1% to 3%. The content of the initiator here refers to the content of the initiator in the isolation film before the liquid is injected.
[0078] In some embodiments, inorganic particles, a binder, a solvent and an initiator are mixed to prepare an inorganic slurry, and an inorganic slurry layer is formed on at least one surface of the porous base film by a coating method, and then dried to obtain an inorganic layer.
[0079] It is understood that the coating method includes but is not limited to blade coating, spin coating, gravure coating and the like.
[0080] It can be understood that the inorganic layer is also disposed on two opposite surfaces of the porous base membrane.
[0081] Furthermore, a pore-forming agent may be added to the inorganic slurry layer, and the pore-forming agent may be removed in the subsequent drying step, thereby playing a role in pore formation.
[0082] As an example, the types of the pore-forming agent include but are not limited to at least one of sodium bicarbonate, ammonium bicarbonate and azo initiators. Azo initiators are easily decomposed by heat to produce nitrogen, so they are easily decomposed during the drying process of the inorganic slurry layer to play a role in pore formation, so they mainly play a role in pore formation here. At the same time, if an azo initiator is used as a pore-forming agent and remains in the inorganic layer, it can also play the role of an initiator in the subsequent curing step of the electrolyte raw material.
[0083] As an example, the azo initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0084] Another embodiment of the present application further provides a method for preparing a secondary battery, comprising the following steps S10 to S20.
[0085] S10, stacking the negative electrode sheet, the separator and the positive electrode sheet to obtain a battery cell;
[0086] S20, injecting electrolyte raw materials into the battery cell, heating and curing in situ, so that the initiator in the above-mentioned isolation film triggers at least part of the electrolyte raw materials to polymerize in situ and form a gel electrolyte; the components of the electrolyte raw materials include electrolyte salt, polymerization monomer and solvent.
[0087] It should be noted that after in-situ curing by heating, the content of initiator in the isolation membrane will change, but there will still be initiator residues in the inorganic layer of the isolation membrane after in-situ polymerization; by performing thermogravimetric analysis or infrared analysis on the inorganic layer samples in the isolation membrane after disassembling the secondary battery, it can be explained that there is initiator in the inorganic layer of the isolation membrane after in-situ polymerization of the secondary battery.
[0088] Traditional gel electrolytes are formed by the following in-situ curing technology: dissolving the initiator in the electrolyte containing the polymerized monomer, injecting the electrolyte for infiltration, and then performing the curing reaction at high temperature. However, the viscosity of the electrolyte system is relatively high, which leads to a slow infiltration rate of the electrolyte. At the same time, the electrolyte does not fully infiltrate the electrode film layer and the isolation film. On the one hand, the slow infiltration rate greatly increases the production cycle of the battery, increases the load and time cost of the subsequent formation equipment, and on the other hand, the insufficient infiltration of the electrolyte in the electrode film layer and the isolation film also greatly affects the power performance of the secondary battery.
[0089] Without wishing to be limited to any theory, the present application pre-sets the initiator in the inorganic layer of the separator, and the initiator may not be added to the electrolyte raw material, so the viscosity of the electrolyte raw material during injection can be reduced to a certain extent, and the electrolyte raw material is fully infiltrated in the battery core. The initiator in the inorganic layer of the separator dissolves and enters the fully infiltrated electrolyte after contact with the electrolyte raw material, and then solidifies under heating conditions, so that a gel electrolyte is formed inside the inorganic layer of the separator and between the separator and the positive electrode and / or the negative electrode. In particular, the gel electrolyte in the inorganic layer can not only improve the flexibility of the inorganic layer and its adhesion to the porous base film, but also improve its ability to transmit ions, thereby improving the power performance of the secondary battery. In addition, the production cycle of the secondary battery is reduced, which is conducive to reducing costs.
[0090] In addition, since the electrolyte is relatively fully injected and infiltrated, the secondary battery can achieve a lower injection coefficient, which is beneficial to improving the energy density of the battery.
[0091] The initiator in the inorganic layer of the separator dissolves and enters the fully infiltrated electrolyte after contacting the electrolyte raw material, and then solidifies at high temperature, so that a gel electrolyte is formed inside the inorganic layer of the separator and between the separator and the positive electrode sheet and / or the negative electrode sheet. In other words, the secondary battery includes the gel electrolyte.
[0092] It can be understood that the gel electrolyte includes an electrolyte salt and a polymer formed by polymerizing the above-mentioned polymerized monomers.
[0093] In some embodiments, the heat curing condition includes curing at a temperature of 50 to 90°C for 4 to 24 hours. The temperature of the heat curing can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, and can be 60 to 70°C, or a range of any two of the above values. The heat curing time can be 4h, 6h, 8h, 10h, 12h, 15h, 18h, 20h, 23h, 24h, and can be 8h to 15h, or a range of any two of the above values.
[0094] In some of the embodiments, the electrolyte raw material is not completely solidified, and the unsolidified part of the electrolyte raw material is also retained in the secondary battery as a liquid electrolyte. It can be understood that the components of the liquid electrolyte include an electrolyte salt and a solvent.
[0095] Further, in the secondary battery, the mass content of the gel electrolyte accounts for the sum of the mass of the gel electrolyte and the liquid electrolyte, that is, the solidification ratio of the electrolyte is 60% to 100%, for example, 60%, 70%, 80%, 90%, 100%. It can be seen that the secondary battery of the present application can maintain a high level of power performance on the basis of a high solidification ratio. Optionally, the solidification ratio of the electrolyte is 60% to 90% or 60% to 80%.
[0096] Further, at least a portion of the liquid electrolyte is located inside at least one of the positive electrode sheet and the negative electrode sheet. It is understood that the liquid electrolyte can also be filled in the gap between the positive electrode sheet and the negative electrode sheet.
[0097] Electrolyte raw materials
[0098] The electrolyte raw material is the electrolyte before injection, and its components include electrolyte salt, polymerized monomer and solvent. After injection and heating and curing, the electrolyte in the secondary battery includes gel electrolyte and optionally liquid electrolyte.
[0099] In some of these embodiments, the liquid electrolyte includes an electrolyte salt and a solvent.
[0100] In some of the embodiments, the gel electrolyte includes an electrolyte salt and a polymer.
[0101] In some embodiments, the electrolyte salt includes at least one of a sodium salt, a lithium salt, and a potassium salt.
[0102] As an example, the sodium salt in the electrolyte salt can be selected from one or more of sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium hexafluorophosphate (NaPF6), sodium hexafluoroarsenate (NaAsF6), sodium trifluoroacetate (CF3COONa), sodium tetraphenylborate (NaB(C6H5)4), sodium trifluoromethylsulfonate (NaSO3CF3), sodium bis(fluorosulfonyl)imide (Na[(FSO2)2N]) or sodium bis(trifluoromethylsulfonyl)imide (Na[(CF3SO2)2N]).
[0103] As an example, the lithium salt in the electrolyte salt can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0104] In some embodiments, the solvent includes at least one of an ether solvent, an ester solvent and a sulfone solvent.
[0105] As an example, the ether solvent may include at least one of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (TRGDME), tetraethylene glycol dimethyl ether (TEGDME), and 1,3-dioxolane (DOL);
[0106] As an example, the ester solvent may include at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), γ-butyrolactone (BL), 1,3-propane sultone (1,3-PS), methyl propionate (MP), methyl butyrate (MB), ethyl acetate (EA), ethyl propionate (EP), propyl propionate (PP) and ethyl butyrate (EB).
[0107] As an example, the sulfone-based solvent includes dimethyl sulfoxide (DMSO).
[0108] Further, the polymerizable monomer used to form the polymer includes a comonomer. In this case, the initiator includes a free radical polymerization initiator.
[0109] As an example, the comonomer includes at least one of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, butyl acrylate, n-octyl methacrylate, n-octyl acrylate, vinyl acetate, vinylene carbonate, acrylonitrile, vinylethylene carbonate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, allyl methacrylate, divinylbenzene, polyvinyl alcohol, hexafluoropropylene, trichloroethylene, tetrafluoroethylene, chlorotrifluoroethylene and styrene.
[0110] In some embodiments, additives may also be included in at least one of the above electrolyte raw materials, gel electrolytes, and liquid electrolytes. For example, the additives may include film-forming additives, plasticizers, and may also include additives that can improve certain battery performance, such as additives for improving the overcharge performance of the battery, additives for improving the high-temperature performance of the battery, additives for improving the low-temperature performance of the battery, and the like. Further, the plasticizer includes at least one of polyethylene glycol (PEG) and the like.
[0111] In some embodiments, inorganic fillers may also be included in at least one of the above electrolyte raw materials, gel electrolytes, and liquid electrolytes.
[0112] Positive electrode plate
[0113] The current collector in the positive electrode plate is the positive current collector, which may be a conventional metal foil or a composite current collector, and the composite current collector may be formed by disposing a metal material on a polymer substrate. As an example, the positive current collector may be an aluminum foil.
[0114] Further, the positive electrode plate further includes a positive electrode film layer provided on at least one surface of the positive current collector, and the positive electrode film layer includes a positive electrode active material.
[0115] The specific type of the positive electrode active material may be an active material known in the art that can be used for the positive electrode of a secondary battery, and those skilled in the art can select according to actual needs.
[0116] As an example, the positive electrode active material may include a sodium ion active material, and the sodium ion active material may be a positive electrode active material known in the art for sodium ion batteries. As an example, the sodium ion active material may include at least one of the following materials: Prussian blue (PBA) type, with the chemical formula (NaxMA[MB(CN)6]·zH2O, where MA and MB are transition metal ions, which is a compound composed of sodium, transition metal, and cyanide group, such as Na4Fe2(CN)6, Na4Fe(CN)6, Na 1.72 MnFe2(CN)6, NaMnMn(CN)6, NaNiFe(CN)6, etc.; oxide type, with the chemical formula NaxMO2, 0 < x ≤ 1, M is a transition metal element, which is composed of transition metal oxides, and the variable valence transition metals involved mainly include vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu), among which manganese and iron with relatively rich resources are most commonly used, such as NaCrO2, NaMnO2, NaMnO2, Na 0.61 Ti 0.48 Mn 0.52 O2, Na[Fe 0.5 Co 0.5]O2, NaMnO2, Na[Ni 0.25 Fe 0.5 Mn 0.25 ]O2, etc.; and polyanionic compound type, the chemical formula is Na x M y [(XO m ) n- ] z , M is a metal ion with a variable valence state, X is an element such as P, S and V, which is composed of sodium, transition metals and anions, among which the transition metals mainly include iron, vanadium, cobalt, etc., and the anions mainly include phosphate, pyrophosphate, fluorophosphate and sulfate, such as NaMnFe2(PO4)6, Na2MnP2O7, Na3V2(PO4)3, Na2Fe2(SO4)3, NaFePO4, Na3V2(PO4)2F3, Na4Co3(PO4)2(P2O7).
[0117] As an example, the positive electrode active material may include a lithium ion active material, which includes, but is not limited to, one or more of lithium transition metal oxides, lithium phosphates with an olivine structure, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of lithium phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and modified compounds thereof. These materials can all be obtained commercially.
[0118] In some embodiments, the modified compounds of the above materials may be doping-modified and / or surface-coated modified materials.
[0119] Any of the above-mentioned positive electrode film layers may also optionally include a binder, a conductive agent and other optional auxiliary agents.
[0120] As an example, the conductive agent may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.
[0121] As an example, the binder can be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).
[0122] In some embodiments, the positive electrode sheet can be prepared by the following method: the raw material components of the positive electrode film layer used to prepare the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained. It is understood that when the positive electrode film layer is multi-layer, it can be carried out multiple times in sequence. The solvent includes but is not limited to N-methylpyrrolidone.
[0123] Negative electrode
[0124] The negative electrode plate includes a negative electrode current collector. Further, the negative electrode plate also includes a negative electrode film layer arranged on at least one surface of the negative electrode current collector.
[0125] Furthermore, the negative electrode film layer includes a negative electrode active material. In another example, the negative electrode film layer may not contain a negative electrode active material, forming a negative electrode sheet without a negative electrode active material.
[0126] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0127] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy; the polymer material substrate includes but is not limited to at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0128] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Further, the silicon oxide compound includes at least one of silicon dioxide and silicon monoxide. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0129] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0130] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0131] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener. For example, the thickener may be sodium carboxymethyl cellulose (CMC-Na).
[0132] In some embodiments, the negative electrode sheet can be prepared by the following method: the raw material components of the negative electrode film layer used to prepare the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent such as deionized water to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. It is understood that when the negative electrode film layer is multi-layer, it can be carried out multiple times in sequence.
[0133] The shape of the secondary battery in the embodiment of the present application can be cylindrical, square or any other shape. Figure 1 The secondary battery 1 is a square structure as an example.
[0134] In some embodiments, reference Figure 2, the outer packaging may include a shell 11 and a cover plate 13. Among them, the shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a accommodating cavity. The shell 11 has an opening connected to the accommodating cavity, and the cover plate 13 can be covered on the opening to close the accommodating cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 12 through a winding process or a lamination process. The electrode assembly 12 is encapsulated in the accommodating cavity. The above-mentioned electrolyte raw materials are infiltrated into the electrode assembly 12 and then heated and cured. The number of electrode assemblies 12 contained in the secondary battery 1 can be one or more, and those skilled in the art can choose according to specific actual needs.
[0135] In addition, the present invention further provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided by the present invention. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.
[0136] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0137] Figure 3 The power consumption device 2 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.
[0138] As another example, the device may be a mobile phone, a tablet computer, a laptop computer, etc.
[0139] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0140] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.
[0141] 1. Battery Preparation
[0142] Example 1
[0143] 1. Positive electrode. Nickel-cobalt-manganese (LiNi 0.98 Co 0.017 Mn 0.003 O3) ternary material, conductive agent carbon black, binder polyvinylidene fluoride (PVDF) in a mass ratio of 97:1:2, add N-methylpyrrolidone, mix and stir for 3 hours to obtain positive electrode slurry; then evenly coat it on the positive electrode current collector aluminum foil, with a coating mass of 30mg / cm 2 After drying, cold pressing and slitting, the positive electrode sheet is obtained.
[0144] 2. Negative electrode sheet. Active material (artificial graphite with a DV50 particle size of 15 μm + SiO (silicon dioxide) with a DV50 particle size of 6 μm, the mass ratio of the two is 4:6), conductive agent carbon black, carbon nanotubes (CNT), binder styrene butadiene rubber (SBR), thickener sodium hydroxymethyl cellulose (CMC), according to the weight ratio of 94.5:1:0.375:2.8:1.325, add to deionized water, mix and stir for 4 hours to obtain negative electrode active slurry. The negative electrode active slurry is evenly coated on the negative electrode current collector copper foil and dried to form a negative electrode film layer.
[0145] 3. Isolation membrane. Take a polyethylene porous base membrane with a thickness of 7μm, a porosity of 40%, and a pore size of 10nm. Mix 70wt% of inorganic particle silica with a Dv50 of 25nm, 28wt% of binder SBR, and 2wt% of initiator to obtain a mixture, and then add 150wt% of the solvent NMP to the mixture to obtain an inorganic layer slurry; apply the inorganic layer slurry to both surfaces of the polyethylene porous base membrane, dry and shape at 80°C, and form inorganic layers respectively.
[0146] 4. Electrolyte.
[0147] LiPF6 is dissolved in a mixed solvent of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1 to prepare an electrolyte with a concentration of 1 mol / L; and then 10 wt% (based on the total mass of the 1 mol / L electrolyte) of a polymerizable monomer methyl methacrylate is added thereto to obtain the product.
[0148] 5. Production of lithium-ion batteries. The positive electrode sheet, separator, and negative electrode sheet are wound in order to obtain a bare cell; the bare cell is placed in a packaging shell, and after drying, the electrolyte is first injected and then cured at 70°C for 6 hours. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0149] Various embodiments and comparative examples
[0150] It is basically the same as Example 1, except that the parameters described in Table 1 are different.
[0151] The inorganic layer slurry of the isolation membrane in Comparative Example 1 does not contain an initiator, which is replaced by an equal amount of solvent; 2 wt % of the same type of initiator as in Example 1 is added to the electrolyte raw material.
[0152] Comparative Example 2 directly uses a polyethylene porous base film to replace the isolation film in Example 1, and then immerses the polyethylene porous base film in the same type of initiator solution (the solvent is acetone), and dries to form an isolation film containing the initiator. According to the mass difference before and after the polyethylene porous base film, it is calculated that the amount of initiator added is 2%.
[0153] 2. Battery performance test
[0154] (I) Energy density test
[0155] 1) The discharge energy measurement of the battery cell is as follows:
[0156] Leave the battery cell at 25°C for 2 hours to ensure that the temperature of the battery cell is 25°C;
[0157] After charging the battery cell to the charging cut-off voltage at 0.1C at 25°C, continue to charge at a constant voltage at the charging cut-off voltage until the current reaches 0.05C and the charging is cut off (where C represents the rated capacity of the battery cell);
[0158] Let the battery cells stand at 25°C for 1 hour;
[0159] At 25°C, discharge the battery cell at 0.1C to the discharge cut-off voltage, and record the total discharge energy as E0;
[0160] 2) Battery cell weight measurement: Place the battery cell on an electronic balance until the weight is stable, and read the battery cell weight value M0;
[0161] 3) Energy density calculation: Battery cell discharge energy E0 / battery cell weight M0 is the energy density of the battery cell.
[0162] (II) Power performance test
[0163] The secondary battery prepared in each embodiment and comparative example was discharged to 2.8V at 0.33C constant current and left standing for 30min; charged to 4.25V at 0.33C constant current and then kept at 0.05C constant voltage until the voltage was stable and left standing for 30min; discharged to 2.8V at 0.33C constant current, at which time the initial capacity C0 was read and left standing for 30min; charged to 4.25V at 0.33C constant current and then kept at 0.05C constant voltage until the voltage was stable and left standing for 30min; discharged to 0.4C0Ah (40%) SOC at 0.33C constant current and left standing for 60min; discharged to 2.8V at 4.5C constant current, and the discharge time of "discharging to 2.8V at 4.5C constant current" was recorded in seconds. The longer the discharge time, the better the power performance.
[0164] (III) Cycle test
[0165] 1) The voltage calibration method is as follows: let the battery cell stand at 25℃ for 2h, ensuring that the temperature of the battery cell is 25℃; charge the battery cell to 4.25V at 0.33C0 at 25℃, and charge at 4.25V constant voltage to a current of 0.05C0; let it stand for 1h; discharge at 0.33C0 to 0.95C0 at 25℃, and record the voltage V1 at this time;
[0166] Let stand for 5 minutes; discharge to 2.0V at 0.33C0 at 25°C; let stand for 5 minutes; charge the battery cell to 0.97C0 at 0.33C0 at 25°C, and record the voltage V2 at this time.
[0167] 2) The cycle test process is as follows: let the battery cell stand at 25℃ for 2h, ensuring that the temperature of the battery cell is 25℃; charge the battery cell at 0.33C0 at 25℃ to voltage V2; let stand for 0.5h; discharge the battery cell at 0.33C0 at 25℃ to voltage V1, and record the capacity at this time as Cn; let stand for 0.5h; repeat steps 2 to 5 until the cycle number n, the capacity after n cycles is Cn', and the capacity retention rate after n cycles is Cn' / Cn=80%. Record the cycle number n at this time.
[0168] (IV) Viscosity test of electrolyte raw materials
[0169] The samples are electrolyte raw materials (injection) of various embodiments and comparative examples. A 18# rotor is fixedly selected with a rotation speed of 70 r / min. The viscosity is tested using a DV-2TLV instrument. The results are shown in Table 1, and the unit is mp*S.
[0170] (V) Electrolyte solidification ratio test
[0171] The solidification ratio of the electrolyte refers to the mass content of the gel electrolyte in the sum of the masses of the gel electrolyte and the liquid electrolyte. The sum of the masses of the gel electrolyte and the liquid electrolyte can be equal to the total mass of the added electrolyte raw materials. The remaining liquid electrolyte after solidification can be transferred by centrifuging the battery and weighing its mass, and then the mass of the gel electrolyte is obtained based on the difference between the total mass of the electrolyte raw materials and the liquid electrolyte.
[0172] Table 1
[0173]
[0174]
[0175] As can be seen from Table 1, the inorganic layer slurry of the isolation membrane in Comparative Example 1 does not contain an initiator, but 2wt% of the same type of initiator as in Example 1 is added to the electrolyte raw material, and the viscosity of the electrolyte raw material is relatively large. Comparative Example 2 directly uses a polyethylene porous base film to impregnate a polyethylene isolation membrane with an initiator addition amount of 2%. The impregnation method is not suitable for industrial-scale production, the production efficiency is low, and the uniformity of the impregnation needs to be improved. According to the results in Table 1, the power performance of Comparative Examples 1 to 2 is significantly lower than that of each embodiment.
[0176] Compared with Comparative Examples 1 to 2, each embodiment has improved power performance and cycle performance while having a higher energy density.
[0177] In Examples 1 to 5, other conditions remain unchanged, and only the mass content of the initiator in the inorganic layer is changed within 1% to 10%, and the curing ratio a is also different accordingly. When the mass content of the initiator in the inorganic layer is 1% to 6%, the power performance and cycle performance obtained by the secondary battery are better, and further 1% to 3%.
[0178] In Example 1 and Examples 6 to 9, other conditions remain unchanged, and only the type of initiator is changed. The secondary battery has excellent power performance and cycle performance while having a relatively high energy density.
[0179] In Example 1 and Examples 10 to 13, other conditions remain unchanged, and only the type of inorganic particles in the inorganic layer is changed, indicating that the type of inorganic particles is selected from SiO2, TiO2, Al2O3, lithium aluminum titanium phosphate or barium titanate, and their secondary batteries can obtain excellent power performance and cycle performance.
[0180] In Example 1 and Examples 14 to 15, other conditions remain unchanged, and only the Dv50 of the inorganic particles in the inorganic layer is changed. The secondary battery obtains excellent power performance and cycle performance on the basis of having a higher energy density.
[0181] In Examples 1 and 16 to 18, other conditions remain unchanged, and only the thickness of the inorganic layer is changed within 1 μm to 4 μm, and the secondary batteries thereof can obtain excellent power performance and cycle performance. When the thickness of the inorganic layer is 2 μm to 4 μm, the power performance and cycle performance obtained by the secondary battery are better.
[0182] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0183] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.
Claims
1. A secondary battery, characterized in that: include: Positive electrode; A negative electrode sheet, arranged opposite to the positive electrode sheet; A separator, disposed between the positive electrode sheet and the negative electrode sheet, the separator comprising a porous base film and an inorganic layer, the components of the inorganic layer comprising inorganic particles and an initiator, and the inorganic layer being disposed on at least one surface of the porous base film; and The gel electrolyte is disposed between the positive electrode plate and the separator, between the negative electrode plate and the separator, and in the inorganic layer of the separator. The initiator can initiate a polymerization reaction to form the gel electrolyte.
2. The secondary battery according to claim 1, wherein: The initiator includes a free radical polymerization initiator; Optionally, the free radical polymerization initiator includes at least one of an anionic and cationic initiator and an organic peroxide initiator; More optionally, the anionic and cationic initiator includes at least one of a persulfate initiator and lithium acetate; more optionally, the organic peroxide initiator includes at least one of benzoyl peroxide, tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide.
3. The secondary battery according to claim 1, wherein: The initiator includes lithium acetate.
4. The secondary battery according to any one of claims 1 to 3, characterized in that: The inorganic particles include at least one of Al oxide, Al nitride, Al fluoride, Si oxide, Si nitride, Si fluoride, Fe oxide, Fe nitride, Fe fluoride, Fe oxyacid salt, Ti oxide, Ti nitride, Ti fluoride, Co oxide, Co nitride, Co fluoride, Ni oxide, Ni nitride, Ni fluoride, Mn oxide, Mn nitride, Mn fluoride, Sn oxide, Sn nitride, Sn fluoride, ZnO, barium titanate and lithium aluminum titanium phosphate; Optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, SiO, SnO2, ZnO, Fe2O3, NiO, CuO, FePO4, barium titanate and lithium aluminum titanium phosphate; More optionally, the inorganic particles include at least one of SiO2, TiO2, Al2O3, barium titanate and lithium aluminum titanium phosphate.
5. The secondary battery according to any one of claims 1 to 3, characterized in that: At least one of the following conditions is met: (1a) The Dv50 particle size of the inorganic particles is 50 nm to 70 nm; (1b) The thickness of the inorganic layer is 1 μm to 4 μm, and can be 2 μm to 4 μm.
6. The secondary battery according to any one of claims 1 to 3, characterized in that: At least one of the following conditions is met: (2a) The thickness of the porous base film is 4 μm to 20 μm, and can be 7 μm to 12 μm; (2b) The average pore size of the porous base membrane is ≤200 nm, and can be selected from 10 nm to 200 nm; (2c) The porosity of the porous base film is 30% to 80%; (2d) The material of the porous base film includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, glass fiber, non-woven fabric and natural fiber.
7. The secondary battery according to any one of claims 1 to 3, characterized in that: The gel electrolyte comprises an electrolyte salt and a polymer; Optionally, the polymerization monomer of the polymer includes at least one of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, butyl acrylate, n-octyl methacrylate, n-octyl acrylate, vinyl acetate, vinylene carbonate, acrylonitrile, vinyl ethylene carbonate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, allyl methacrylate, divinylbenzene, polyvinyl alcohol, hexafluoropropylene, trichloroethylene, tetrafluoroethylene, chlorotrifluoroethylene and styrene.
8. The secondary battery according to any one of claims 1 to 3, characterized in that: The secondary battery further comprises a liquid electrolyte, and the mass content of the gel electrolyte accounts for 60% to 100% of the total mass of the gel electrolyte and the liquid electrolyte, and can be 60% to 90%, and more preferably 60% to 80%.
9. A method for preparing a secondary battery, characterized in that: The steps include: forming an inorganic layer on at least one surface of the porous base film, wherein the components of the inorganic layer include inorganic particles and an initiator, to obtain a separator; The negative electrode sheet, the separator and the positive electrode sheet are stacked and assembled to obtain a battery cell; Electrolyte raw materials are injected into the battery core and heated for in-situ curing, so that the initiator triggers at least a portion of the electrolyte raw materials to polymerize in-situ and form a gel electrolyte; the components of the electrolyte raw materials include electrolyte salt, polymerization monomers and solvent.
10. The method for preparing a secondary battery according to claim 9, characterized in that: At least one of the following conditions is met: (3a) the electrolyte salt comprises at least one of a sodium salt, a lithium salt and a potassium salt; (3b) The solvent includes at least one of an ether solvent, an ester solvent and a sulfone solvent.
11. A separation film, characterized in that: The isolation membrane includes a porous base membrane and an inorganic layer. Components of the inorganic layer include inorganic particles and an initiator. The inorganic layer is arranged on at least one surface of the porous base membrane.
12. The isolation film according to claim 11, characterized in that The mass content of the initiator in the inorganic layer is 1% to 10%, optionally 1% to 6%, and more optionally 1% to 3%.
13. An electrical device, characterized in that: The electrical device comprises the secondary battery according to any one of claims 1 to 8 or the secondary battery prepared by the preparation method according to any one of claims 9 to 10.
Citation Information
Cited By
Battery, preparation method thereof and power utilization device
CN121642210A
Battery, method for manufacturing the same, and electric device
CN121642210B
Battery cell and preparation method therefor, battery device and electric device
WO2026174999A1