Adsorption material for treating antibiotics in wastewater as well as preparation method and application of adsorption material
The phenylacetylene copper/peryleneimide composite formed by hydrothermal reaction solves the problems of complex processes and poor stability of existing carbon-based adsorption materials, and achieves efficient removal and stable adsorption effect of antibiotics in wastewater.
Patent Information
- Application Number
- CN202411502284.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-25
AI Technical Summary
The preparation process of existing carbon-based adsorbent materials is cumbersome and susceptible to external environmental factors, resulting in poor adsorption performance stability and making it difficult to promote large-scale production and use.
The composite material is formed by hydrothermal reaction between phenylacetylene copper and nanoperyleneimide, which simplifies the process flow, increases the specific surface area and active sites, and forms a phenylacetylene copper/peryleneimide composite material with excellent adsorption properties.
It has achieved efficient removal of antibiotics in wastewater, the material stability is not affected by external factors such as light and pH, and the adsorption capacity is significantly improved, making it suitable for large-scale production and application.
Smart Images

Figure CN119075957A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antibiotic adsorption materials, and in particular to an adsorption material for treating antibiotics in wastewater, and a preparation method and application thereof. Background Art
[0002] The widespread use and even abuse of antibiotics has led to a wide variety of antibiotics in the environment, which are highly polluting, complex in composition, and extremely difficult to degrade naturally. Antibiotics can enter the food chain through enrichment. They pose a great threat to humans and other organisms and are highly ecologically harmful. Low doses of antibiotics discharged into the environment for a long time can also increase the drug resistance of sensitive bacteria. In addition, drug-resistant genes can expand and evolve in the environment, posing a potential threat to the ecological environment and human health. Therefore, removing antibiotic pollutants has become a very urgent task.
[0003] At present, common methods for removing antibiotics include adsorption, membrane separation, photocatalysis and biodegradation. Among them, adsorption is considered to be one of the most promising methods for removing antibiotics because of its low cost, simple operation, wide applicability and no secondary pollution.
[0004] High-performance adsorbents are the key to removing antibiotic pollutants from water environments by adsorption. However, the adsorbents used in the prior art are mostly carbon-based adsorbent materials, and the prior art mainly uses high-temperature pyrolysis to prepare carbon-based adsorbent materials, that is, the carbon source is activated, modified, and pyrolyzed in sequence to obtain the carbon-based adsorbent material. The above-mentioned preparation method is processed in sequence through the above-mentioned multiple treatments. Although it can improve the surface functional groups, pores and specific surface area of the carbon material, thereby improving the adsorption of antibiotics, the processing technology of the above-mentioned preparation method is cumbersome, time-consuming and labor-intensive, which is not conducive to promotion for large-scale production and use; and the prepared carbon-based adsorbent material is easily affected by external environmental factors such as pH and light, and the adsorption performance stability is poor. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides an adsorption material for treating antibiotics in wastewater, and a preparation method and application thereof.
[0006] The adsorption material for treating antibiotics in wastewater of the present invention and its preparation method and application are realized by the following technical scheme:
[0007] The present invention takes into account that perylene imide plays an important role in removing pollutants, but the existing technology currently mainly removes pollutants by combining perylene imide with other materials as a photocatalytic material. For example, the prior art "Incorporating Fe, Co co-doped graphene with PDI supermolecular for promoted photocatalytic activity: A story of electron transfer, DOI: 10.1016 / j.jcis.2022.12.145" proposes a method of combining graphene co-doped with Fe and Co with perylene imide supramolecular, so that the iron-cobalt double single atoms are anchored on nitrogen-doped graphene to improve the migration and separation efficiency of photogenerated carriers, and then self-assemble with perylene imide to form a composite material through π-π interaction. Although the above method improves the removal effect of the material on pollutants, the composite material mainly realizes synergistic interaction through the Fe-Co dual active sites, promotes electron transfer in the catalytic reaction, and then realizes photocatalytic degradation of pollutants, that is, the material prepared by the above method is still limited by the external environmental factors of light.
[0008] In order to provide an adsorbent material that is not restricted by external environmental factors such as light, the present invention proposes a method for preparing an adsorbent material for treating antibiotics in wastewater, which specifically comprises the following steps:
[0009] Copper phenylacetylene and nano-perylene imide are dispersed in an organic solvent, and then a hydrothermal reaction is carried out at a temperature of 80°C to 220°C to obtain a copper phenylacetylene / perylene imide composite material. The copper phenylacetylene / perylene imide composite material is used as an adsorption material for treating antibiotics in wastewater.
[0010] It should be noted that, in order to further improve the removal effect of perylene imide on pollutants, the present invention uses phenylacetylene copper as a raw material, and forms a phenylacetylene copper / perylene imide composite material with a high specific surface area by allowing phenylacetylene copper and nanoperylene imide to be supramolecularly combined during a hydrothermal reaction, and the preparation method is simple and easy to operate. The present invention greatly improves the adsorption capacity of phenylacetylene copper for antibiotics in wastewater by compounding phenylacetylene copper on the basis of perylene imide; and the composite phenylacetylene copper / perylene imide composite material is not limited by external environmental factors such as light, has excellent adsorption performance and stability, and can directly achieve efficient removal of antibiotics in wastewater through its own adsorption, so that it can be used as an adsorption material for treating antibiotics in wastewater.
[0011] In some preferred embodiments of the present invention, the mass ratio of the copper phenylacetylene and the nano-perylene imide is 1:0.1-10, so as to ensure that the added copper phenylacetylene and the nano-perylene imide can fully react to form a copper phenylacetylene / perylene imide composite material, and the obtained copper phenylacetylene / perylene imide composite material has the best adsorption effect and stable performance under different pH values.
[0012] In some preferred embodiments of the present invention, the organic solvent is one or more of an alcohol solvent and N,N-dimethylformamide. This ensures that the organic solvent used has good solubility or dispersibility for both phenylacetylene copper and nano-perylene imide, thereby facilitating full contact and reaction between phenylacetylene copper and nano-perylene imide in the organic solvent. Among them, in some more preferred embodiments of the present invention, the alcohol solvent is one or more of ethanol, methanol and ethylene glycol.
[0013] In some preferred embodiments of the present invention, the usage ratio of the organic solvent to the copper phenylacetylene is 10 mL to 100 mL: 15 mg to 120 mg, so that the added organic solvent can fully dissolve or disperse the copper phenylacetylene and nano-perylene imide.
[0014] In some preferred embodiments of the present invention, the copper phenylacetylene and the nano-perylene imide are dispersed in an organic solvent by first stirring and then ultrasonically treating, so that the copper phenylacetylene and the nano-perylene imide are quickly and evenly dispersed or dissolved in the organic solvent. In some preferred embodiments of the present invention, when ultrasonic treatment is performed, the power of the ultrasonic treatment is 50W to 300W, and the ultrasonic time is 2min to 100min. In some other preferred embodiments of the present invention, the stirring treatment is performed, and the stirring treatment time is 20min to 180min.
[0015] In some preferred embodiments of the present invention, the hydrothermal reaction time is 1 h to 16 h, so that the reaction of copper phenylacetylene and perylene imide is more complete.
[0016] The present invention also provides an adsorption material prepared by the above preparation method of the present invention.
[0017] The present invention also provides an application of the adsorption material prepared by the preparation method of the present invention in adsorbing antibiotics in waste water.
[0018] It should be noted that when the adsorbent material prepared by the above-mentioned preparation method of the present invention is used to adsorb antibiotics in wastewater, the adsorbent material of the present invention is placed in the wastewater to be treated, and then treated by ultrasound, so that the adsorbent material is fully in contact with and adsorbs the antibiotics in the wastewater to be treated through the ultrasonic action, thereby achieving the removal of the antibiotics in the wastewater to be treated.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention utilizes a simple one-step hydrothermal method to successfully compound phenylacetylene copper on the basis of perylene imide, and phenylacetylene copper and nanoperylene imide are supermolecularly combined during the hydrothermal reaction process to form an adsorbent material with a high specific surface area for treating antibiotics in wastewater, namely, phenylacetylene copper / perylene imide composite material. The preparation method of the present invention is simple and easy to operate, simplifies the process flow and preparation difficulty of the adsorbent material, and is conducive to promotion and large-scale production and use.
[0021] The copper phenylacetylene / perylene imide composite material prepared by the present invention has abundant active sites, strong π-π stacking force and high adsorption capacity; and the copper phenylacetylene / perylene imide composite material prepared by the present invention is not affected by external environmental factors such as pH and light, and has excellent adsorption performance stability. Compared with a single copper phenylacetylene and a single perylene imide, the present invention can effectively improve the adsorption capacity of the material for adsorbing antibiotics in wastewater by compounding copper phenylacetylene and perylene imide; and the obtained copper phenylacetylene / perylene imide composite material is not limited by external environmental factors such as light, and can directly achieve efficient removal of antibiotics in wastewater through its own adsorption, so that it can be used as an adsorption material for treating antibiotics in wastewater. In addition, new basic copper carbonate was generated during the hydrothermal reaction of copper phenylacetylene and nano-perylene imide. The generation of basic copper carbonate enabled perylene imide and copper phenylacetylene to be successfully composited. On the one hand, the specific surface area of the perylene imide and copper phenylacetylene composite material was greatly increased, and the pore size and pore volume were increased; on the other hand, the introduction of the Cu element also provided more abundant active sites for the copper phenylacetylene / perylene imide composite material, further improving the adsorption performance of the copper phenylacetylene / perylene imide composite material.
[0022] When the phenylacetylene copper / perylene imide composite material prepared by the present invention is used as an adsorption material, it can achieve adsorption of target antibiotic pollutants in wastewater without the need for special illumination or specific pH conditions, and is not affected by external environmental factors such as illumination or pH. Moreover, the maximum adsorption amount of tetracycline of the adsorption material of the present invention can reach 238.33 mg / g under ultrasound for 30 minutes, which is 21.96 times and 12.36 times the maximum adsorption amount of tetracycline of single phenylacetylene copper and single perylene imide, respectively. Moreover, the adsorption removal rate of ciprofloxacin prepared by the present invention can also reach 81.97%, indicating that when the phenylacetylene copper / perylene imide composite material prepared by the present invention is used as an adsorption material, it has good adsorption versatility for antibiotics in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the scanning electron microscope image of phC2Cu of Comparative Example 1.
[0024] Figure 2 This is the PDI scanning electron microscope image of Comparative Example 2.
[0025] Figure 3 This is the scanning electron microscope image of phC2Cu / PDI of Example 1.
[0026] Figure 4 It is the EDS energy spectrum diagram of phC2Cu / PDI of Example 1. In the figure, Figure a is the EDS total element distribution diagram of phC2Cu / PDI of Example 1, Figure b is the distribution diagram of C element in Figure a, Figure c is the distribution diagram of O element in Figure a, Figure d is the distribution diagram of Cu element in Figure a, and Figure e is the distribution diagram of N element in Figure a.
[0027] Figure 5 These are the XRD spectra of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1.
[0028] Figure 6 This is the XPS spectrum of phC2Cu / PDI of Example 1. In the figure, Figure a is the C 1s spectrum of phC2Cu / PDI, Figure b is the N1s spectrum of phC2Cu / PDI, Figure c is the O1s spectrum of phC2Cu / PDI, and Figure d is the Cu 2p spectrum of phC2Cu / PDI.
[0029] Figure 7 These are the N2 adsorption-desorption isotherms of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1.
[0030] Figure 8 Pore size distribution curves of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1.
[0031] Fig. 9 Cumulative pore volume distribution curves of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1.
[0032] Fig.10 The adsorption performance test results of phC2Cu / PDI in Example 1 for tetracycline and ciprofloxacin.
[0033] Fig.11 FTIR spectra of phC2Cu before and after adsorption in Example 1. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below.
[0035] Example 1
[0036] This embodiment provides an adsorbent material for treating antibiotics in wastewater, which is prepared by the following steps:
[0037] Step 1, preparation of nanoperylene imide:
[0038] 1.1) Under nitrogen protection, 1.376 g of 3,4,9,10-perylenetetracarboxylic dianhydride, 2.5 g of 3-aminopropionic acid and 16 g of imidazole were mixed, and the mixture was reacted at 100° C. for 4 h. After the reaction was completed, the mixture was cooled to room temperature, 100 mL of ethanol and 300 mL of 2 M hydrochloric acid were added, and the mixture was reacted for 12 h under stirring to obtain a red solution.
[0039] 1.2) The obtained red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain a crude perylene imide.
[0040] 1.3) Disperse 0.54 g of crude perylene imide in 200 mL of deionized water, add 800 μL of triethylamine and stir for 1 h; then add 35 mL of 2 M hydrochloric acid and stir for 3 h to obtain a dark red solution.
[0041] 1.4) The obtained dark red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain nanoperylene imide.
[0042] Step 2, Preparation of Copper Phenylacetylene
[0043] 2.1) Mix 0.365 g of cupric chloride dihydrate with 40 mL of methanol to obtain a methanol solution of cupric chloride.
[0044] 2.2) Add 1.12 mL of triethylamine to the above copper chloride methanol solution and stir evenly; then, add 0.44 mL of phenylacetylene and mix evenly, then transfer to a 65°C water bath and stir for 30 minutes.
[0045] 2.3) The reaction solution obtained in 2.2) above was filtered, washed with deionized water and anhydrous ethanol, and the solid was collected and dried in a vacuum drying oven at 60° C. for 12 h to obtain phenylacetylene copper.
[0046] Step 3, hydrothermal reaction:
[0047] 3.1) 0.1 g of the nanoperylene imide obtained in step 1.4) and 0.02 g of the copper phenylacetylene obtained in step 2.3) were placed in 40 mL of ethanol and stirred for 120 min to obtain a stirred mixed solution.
[0048] 3.2) The obtained stirred mixed solution was ultrasonically treated at an ultrasonic power of 200 W for 30 min to obtain an ultrasonic mixed solution.
[0049] 3.3) The ultrasonic mixed solution was transferred to a 50 mL polytetrafluoroethylene liner, sealed in a reaction kettle, and the reaction kettle was placed in an oven for hydrothermal reaction at 120° C. for 12 h.
[0050] 3.4) The reaction solution obtained in 3.3) above was centrifugally washed three times with anhydrous ethanol, and the washed material was placed in a vacuum drying oven and dried at 60° C. for 12 h to obtain a phenylacetylene copper / perylene diimide composite material, recorded as phC2Cu / PDI.
[0051] Example 2
[0052] This embodiment provides an adsorbent material for treating antibiotics in wastewater, which is prepared by the following steps:
[0053] Step 1, preparation of nanoperylene imide:
[0054] 1.1) Under nitrogen protection, 1.376 g of 3,4,9,10-perylenetetracarboxylic dianhydride, 2.5 g of 3-aminopropionic acid and 16 g of imidazole were mixed, and the mixture was reacted at 100° C. for 4 h. After the reaction was completed, the mixture was cooled to room temperature, 100 mL of ethanol and 300 mL of 2 M hydrochloric acid were added, and the mixture was reacted for 12 h under stirring to obtain a red solution.
[0055] 1.2) The obtained red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain a crude perylene imide.
[0056] 1.3) Disperse 0.54 g of crude perylene imide in 200 mL of deionized water, add 800 μL of triethylamine and stir for 1 h; then add 35 mL of 2 M hydrochloric acid and stir for 3 h to obtain a dark red solution.
[0057] 1.4) The obtained dark red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain nanoperylene imide.
[0058] Step 2, Preparation of Copper Phenylacetylene
[0059] 2.1) Mix 0.365 g of cupric chloride dihydrate with 40 mL of methanol to obtain a methanol solution of cupric chloride.
[0060] 2.2) Add 1.12 mL of triethylamine to the above copper chloride methanol solution and stir evenly; then, add 0.44 mL of phenylacetylene and mix evenly, then transfer to a 65°C water bath and stir for 30 minutes.
[0061] 2.3) The reaction solution obtained in 2.2) above was filtered, washed with deionized water and anhydrous ethanol, and the solid was collected and dried in a vacuum drying oven at 60° C. for 12 h to obtain phenylacetylene copper.
[0062] Step 3, hydrothermal reaction:
[0063] 3.1) 0.006 g of the nanoperylene imide obtained in step 1.4) and 0.06 g of the copper phenylacetylene obtained in step 2.3 were placed in 10 mL of ethanol and stirred for 180 min to obtain a stirred mixed solution.
[0064] 3.2) The obtained stirred mixed solution was ultrasonically treated at an ultrasonic power of 50 W for 100 min to obtain an ultrasonic mixed solution.
[0065] 3.3) The ultrasonic mixed solution was transferred to a polytetrafluoroethylene liner, sealed in a reaction kettle, and the reaction kettle was placed in an oven for hydrothermal reaction at 80°C for 8h.
[0066] 3.4) The reaction solution obtained in 3.3) was washed three times by centrifugation with anhydrous ethanol, and the washed material was placed in a vacuum drying oven and dried at 60° C. for 12 h to obtain a phenylacetylene copper / perylene imide composite material.
[0067] Example 3
[0068] This embodiment provides an adsorbent material for treating antibiotics in wastewater, which is prepared by the following steps:
[0069] Step 1, preparation of nanoperylene imide:
[0070] 1.1) Under nitrogen protection, 1.376 g of 3,4,9,10-perylenetetracarboxylic dianhydride, 2.5 g of 3-aminopropionic acid and 16 g of imidazole were mixed, and the mixture was reacted at 100° C. for 4 h. After the reaction was completed, the mixture was cooled to room temperature, 100 mL of ethanol and 300 mL of 2 M hydrochloric acid were added, and the mixture was reacted for 12 h under stirring to obtain a red solution.
[0071] 1.2) The obtained red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain a crude perylene imide.
[0072] 1.3) Disperse 0.54 g of crude perylene imide in 200 mL of deionized water, add 800 μL of triethylamine and stir for 1 h; then add 35 mL of 2 M hydrochloric acid and stir for 3 h to obtain a dark red solution.
[0073] 1.4) The obtained dark red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain nanoperylene imide.
[0074] Step 2, Preparation of Copper Phenylacetylene
[0075] 2.1) Mix 0.365 g of cupric chloride dihydrate with 40 mL of methanol to obtain a methanol solution of cupric chloride.
[0076] 2.2) Add 1.12 mL of triethylamine to the above copper chloride methanol solution and stir evenly; then, add 0.44 mL of phenylacetylene and mix evenly, then transfer to a 65°C water bath and stir for 30 minutes.
[0077] 2.3) The reaction solution obtained in 2.2) above was filtered, washed with deionized water and anhydrous ethanol, and the solid was collected and dried in a vacuum drying oven at 60° C. for 12 h to obtain phenylacetylene copper.
[0078] Step 3, hydrothermal reaction:
[0079] 3.1) 1.2 g of the nanoperylene imide obtained in step 1.4) and 0.12 g of the copper phenylacetylene obtained in step 2.3 were placed in 100 mL of ethanol and stirred for 20 min to obtain a stirred mixed solution.
[0080] 3.2) The obtained stirred mixed solution was ultrasonically treated at an ultrasonic power of 300 W for 20 min to obtain an ultrasonic mixed solution.
[0081] 3.3) The ultrasonic mixed solution was transferred to a polytetrafluoroethylene liner, sealed in a reaction kettle, and the reaction kettle was placed in an oven for hydrothermal reaction at 220° C. for 1 h.
[0082] 3.4) The reaction solution obtained in 3.3) was washed three times by centrifugation with anhydrous ethanol, and the washed material was placed in a vacuum drying oven and dried at 60° C. for 12 h to obtain a phenylacetylene copper / perylene imide composite material.
[0083] Comparative Example 1
[0084] This comparative example provides an adsorption material for treating antibiotics in wastewater, which is prepared by the following steps:
[0085] 1) Mix 0.365 g of cupric chloride dihydrate with 40 mL of methanol to obtain a methanol solution of cupric chloride.
[0086] 2) Add 1.12 mL of triethylamine to the above copper chloride methanol solution and stir evenly; then, add 0.44 mL of phenylacetylene and mix evenly, then transfer to a 65°C water bath and stir to react for 30 minutes.
[0087] 3) The reaction solution obtained in the above 2) was filtered, washed with deionized water and anhydrous ethanol, and the solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain phenylacetylene copper, which was recorded as phC2Cu.
[0088] That is, the difference between this comparative example and Example 1 is only that:
[0089] No hydrothermal reaction was carried out with perylene imide, that is, in this comparative example, single copper phenylacetylene was used as the adsorption material.
[0090] Comparative Example 2
[0091] This comparative example provides an adsorption material for treating antibiotics in wastewater, which is prepared by the following steps:
[0092] 1) Under nitrogen protection, 1.376 g of 3,4,9,10-perylenetetracarboxylic dianhydride, 2.5 g of 3-aminopropionic acid and 16 g of imidazole were mixed and reacted at 100° C. for 4 h. After the reaction was completed, the mixture was cooled to room temperature, 100 mL of ethanol and 300 mL of 2 M hydrochloric acid were added, and then the mixture was reacted for 12 h under stirring to obtain a red solution.
[0093] 2) The obtained red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain a crude product of perylene imide.
[0094] 3) Take 0.54 g of crude perylene imide and disperse it in 200 mL of deionized water, add 800 μL of triethylamine and stir for 1 h; then add 35 mL of 2 M hydrochloric acid and stir for 3 h to obtain a dark red solution.
[0095] 4) The obtained dark red solution was filtered through a 0.45 μm filter membrane and washed with distilled water until the pH value was neutral. The solid was collected and dried in a vacuum oven at 60° C. for 12 h to obtain nano-perylene diimide, which was recorded as PDI.
[0096] That is, the difference between this comparative example and Example 1 is only that:
[0097] No hydrothermal reaction was carried out with copper phenylacetylene, that is, in this comparative example, a single perylene imide was used as the adsorption material.
[0098] Experimental Section
[0099] (I) Scanning electron microscope test
[0100] The present invention takes the phC2Cu of comparative example 1, the PDI of comparative example 2 and the phC2Cu / PDI of embodiment 1 as examples, and performs scanning electron microscope tests on them respectively, and the test results are as follows: Figure 1 to Figure 3 shown.
[0101] Figure 1 This is the scanning electron microscope image of phC2Cu of comparative example 1. It can be seen that the sample grows into a longer nanobelt structure and accumulates into bundles, which can provide more adsorption sites for the adsorption of the target.
[0102] Figure 2 This is the scanning electron microscope image of PDI in comparative example 2. It can be seen that pure PDI presents the morphology of one-dimensional microrods.
[0103] Figure 3 The scanning electron microscope image of phC2Cu / PDI in Example 1 shows that the samples all show a regular rod-like structure with a relatively uniform distribution. Figure 1 and 2 As for the phC2Cu / PDI of Example 1, due to the introduction of Cu element, it will help to provide more abundant active sites, greatly increase the specific surface area of the composite material, and solve the problem of low adsorption capacity of pure nano-PDI and phenylacetylene copper.
[0104] (II) EDS spectrum test
[0105] The present invention takes phC2Cu / PDI of Example 1 as an example and tests it separately, and the test results are as follows Figure 4 In the figure, Figure a is the EDS distribution diagram of each element of phC2Cu / PDI in Example 1, Figure b is the distribution diagram of the C element in Figure a, Figure c is the distribution diagram of the O element in Figure a, Figure d is the distribution diagram of the Cu element in Figure a, and Figure e is the distribution diagram of the N element in Figure a.
[0106] from Figure 4 As can be seen from Figure a, the phC2Cu / PDI prepared in Example 1 is mainly composed of C, O, Cu and N elements. Figure 4 As can be seen from Figures b-e in the figure, C, O, Cu and N elements are evenly distributed on the surface of phC2Cu / PDI prepared in Example 1, indicating that the components of the phenylacetylene copper / perylene imide composite material prepared by the preparation method of the present invention are evenly distributed, which is conducive to ensuring the stability of material performance. And the uniform doping of Cu element in phC2Cu / PDI prepared in Example 1 helps to provide more abundant active sites, thereby solving the problem of low adsorption capacity of pure nano PDI.
[0107] (III) XRD test
[0108] The present invention takes the phC2Cu of comparative example 1, the PDI of comparative example 2 and the phC2Cu / PDI of embodiment 1 as examples, and performs XRD tests respectively, and the test results are as follows: Figure 5 shown.
[0109] Figure 5 The XRD spectra of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1 are shown in FIG. Figure 5 It can be seen that the peaks between 24° and 28° are due to the typical π-π stacking between PDI skeletons. Obviously, the intensity of the 14° peak in the phC2Cu / PDI sample is lower than that of the 26° peak. Similar to nano-PDI, the peak intensity ratio of the 26° peak to the 14° peak is greater than 1, proving that phC2Cu / PDI has a strong π-π stacking force, which indirectly proves that the composite adsorbent has a good adsorption effect, and the π-π stacking also plays a certain role.
[0110] (IV) XPS test
[0111] The present invention takes the phC2Cu / PDI of Example 1 as an example and performs an X-ray photoelectron spectroscopy (XPS) test on it, and the test results are as follows: Figure 6 shown.
[0112] Figure 6 is the XPS spectrum of phC2Cu / PDI of Example 1, Figure 6 In the figure, Figure a is the C1s spectrum of phC2Cu / PDI, Figure b is the N1s spectrum of phC2Cu / PDI, Figure c is the O1s spectrum of phC2Cu / PDI, and Figure d is the Cu 2p spectrum of phC2Cu / PDI.
[0113] Depend on Figure 6 It can be seen from Figures a-d in the figure that C, O, Cu and N elements are indeed present in phC2Cu / PDI of Example 1.
[0114] And by Figure 6 In Figure a, four characteristic peaks with different binding energies can be observed: 284.79eV, 285.42eV, 287.84eV, and 288.77eV. The peaks at 288.77eV and 285.42eV correspond to the OC=O bond in PDI and the C≡C bond in phC2Cu, respectively. The peak at 287.84eV indicates the presence of metal carbonate, further confirming the successful binding of phC2Cu with PDI.
[0115] And by Figure 6In Figure b, three characteristic peaks can be observed, with binding energies at 399.44, 400.09, and 400.82 eV, respectively. Among them, the peaks at 400.09 eV and 400.82 eV correspond to CN in PDI. X group, while the peak at 399.44 eV corresponds to the NH bond in PDI.
[0116] And by Figure 6 A characteristic peak can be observed in Figure c, and this characteristic peak can be further decomposed into two peaks. The peak at a binding energy of 533.36 eV is attributed to the C=O group in PDI, while the peak at 531.52 eV proves the presence of metal carbonate.
[0117] And by Figure 6 Four characteristic peaks can be observed in the d graph, which are located at 933.12eV, 934.9eV, 952.88eV and 954.42eV. Among them, the peaks at 933.12eV and 952.88eV are Cu 2p 3 / 2 and Cu 2p 1 / 2 The peaks at 934.9eV and 954.42eV are consistent with the above findings, and it is speculated that basic copper carbonate is generated during the combination of these two materials. These results fully demonstrate the successful combination of phC2Cu and PDI.
[0118] (V) BET test
[0119] The present invention takes phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1 as examples, and tests are performed on their pore structures, and the test results are as follows: Figure 7-Figure 9 shown.
[0120] Figure 7 The N2 adsorption-desorption isotherms of phC2Cu of comparative example 1, PDI of comparative example 2 and phC2Cu / PDI of example 1 show that the isotherms of PDI, phC2Cu and phC2Cu / PDI all belong to type IV, which is a mesoporous material. The specific surface area of phC2Cu / PDI (95.6062 m 2 g -1 ) is much larger than PDI (0.4992m 2 g -1 ) and phC2Cu(51.377m 2 g -1 ).
[0121] Figure 8The pore size distribution curves of phC2Cu of comparative example 1, PDI of comparative example 2 and phC2Cu / PDI of example 1 show that, relative to comparative example 2, the pore size of phC2Cu / PDI of example 1 has changed significantly, and the pore size has increased significantly, thereby effectively improving the specific surface area of the material. This is one of the reasons for enhancing the adsorption performance of the new material.
[0122] Fig. 9 The cumulative pore volume distribution curves of phC2Cu of Comparative Example 1, PDI of Comparative Example 2 and phC2Cu / PDI of Example 1 show that the cumulative pore volume is significantly increased, which is one of the reasons for enhancing the adsorption performance of the new material.
[0123] (VI) Adsorption performance test
[0124] 1) Test on the adsorption performance of tetracycline in solution
[0125] The present invention uses phC2Cu / PDI of Example 1 as the adsorption material, and tests its adsorption performance respectively, and the test method is:
[0126] Weigh 20 mg of phC2Cu / PDI of Example 1 and place it in a 250 mL beaker, add 100 mL of the initial tetracycline solution with a mass concentration of 20 mg / L, i.e., TC solution, transfer it to a temperature-controlled ultrasonic machine, and keep ultrasonic at 25°C for 30 minutes. Pipette the supernatant every 6 minutes and filter it with a 0.22 μm mixed cellulose microporous filter membrane. The filtrate obtained is the TC solution after adsorption equilibrium. Measure the absorbance of the obtained filtrate at the maximum absorption wavelength of 357 nm. Calculate the mass concentration of the TC solution after adsorption equilibrium based on the mass concentration of the TC solution and the absorbance measurement curve fitting equation, and calculate the equilibrium adsorption capacity of phC2Cu / PDI by formula 1. Among them, the mass concentration of the TC solution and the absorbance measurement curve fitting equation are y1=0.0329x1-0.0034, R 2 =0.999, where x1 is the mass concentration of TC solution, mg / L; y1 is the absorbance at the maximum absorption wavelength of 357 nm.
[0127]
[0128] In the formula, q e1 is the equilibrium adsorption capacity of phC2Cu / PDI, mg / g; C 01 is the initial mass concentration of TC solution, 20 mg / L; C e1 is the mass concentration of TC in the solution when the adsorption reaches equilibrium, mg / L; V1 is the total volume of the solution, 100 mL; m1 is the mass of the adsorbent phC2Cu / PDI, 20 mg.
[0129] 2) Test on the adsorption performance of ciprofloxacin in solution
[0130] The present invention is tested according to the above method, replacing the above tetracycline solution with a mass concentration of 20 mg / L with a ciprofloxacin solution with a mass concentration of 20 mg / L, i.e., a CIP solution, and the difference in the test is that:
[0131] The absorbance of the obtained filtrate at the maximum absorption wavelength of 272 nm was measured, and the mass concentration of the CIP solution after the measured adsorption equilibrium was calculated according to the mass concentration of the CIP solution and the absorbance measurement curve fitting equation, and the equilibrium adsorption capacity of phC2Cu / PDI was calculated by formula 2. Among them, the mass concentration of the CIP solution and the absorbance measurement curve fitting equation are y2=0.0815x2-0.0128, R 2 =0.9994, where x2 is the mass concentration of the CIP solution, mg / L; y2 is the absorbance at the maximum absorption wavelength of 272 nm.
[0132]
[0133] In the formula, q e2 is the equilibrium adsorption capacity of phC2Cu / PDI, mg / g; C 02 is the initial mass concentration of CIP solution, 20 mg / L; C e2 is the mass concentration of CIP in the solution when the adsorption reaches equilibrium, mg / L; V2 is the total volume of the solution, 100 mL; m2 is the mass of the adsorbent phC2Cu / PDI, 20 mg.
[0134] The test results of the adsorption performance test of tetracycline in solution and the adsorption performance test of tetracycline in solution are as follows Fig.10 shown.
[0135] according to Fig.10 It can be seen from the test results that when the copper phenylacetylene / perylene imide composite material prepared by the present invention is used as an adsorption material, the maximum adsorption amount of tetracycline can reach 238.33 mg / g when treated under ultrasound for 30 minutes, which is 21.96 times and 12.36 times that of copper phenylacetylene and perylene imide, respectively.
[0136] It can also be seen that when the copper phenylacetylene / perylene imide composite material prepared by the present invention is used as an adsorption material, the adsorption rate of 20 mg / L ciprofloxacin can also reach 81.97%.
[0137] Moreover, the structure of the copper phenylacetylene / perylene imide composite material obtained in Example 2 and Example 3 is similar to that in Example 1, and tests show that the copper phenylacetylene / perylene imide composite material obtained in Example 2 and Example 3 has an adsorption effect on tetracycline of 97% to 99% of that in Example 1; and an adsorption effect on ciprofloxacin of 95% to 97% of that in Example 1.
[0138] The above test results show that the copper phenylacetylene / perylene imide composite material prepared by the present invention can be used as an adsorption material for antibiotics in wastewater, has good adsorption performance and versatility for antibiotics in wastewater, and provides a new idea and option for the treatment of antibiotic wastewater.
[0139] (VII) FTIR test
[0140] The present invention also conducted FTIR tests on the phC2Cu of Example 1 before and after the above-mentioned adsorption performance test, and the test results are as follows: Fig.11 shown.
[0141] Fig.11 The FTIR spectra before and after phC2Cu adsorption of Example 1 are shown in FIG. 1 , wherein the upper spectrum is the FTIR spectrum before phC2Cu adsorption of Example 1, and the lower spectrum is the FTIR spectrum after phC2Cu adsorption of Example 1. Fig.11 As can be seen, 1691cm -1 The peak at 1656 cm is attributed to the stretching vibration of C=O in the carboxyl group. -1 The stretching vibration peak at 1344 cm-1 is caused by the ketone functional group in perylene imide. -1 and 1590cm -1 The absorption peak is attributed to the stretching vibration of -COO-. By comparing the infrared spectra before and after adsorption, it can be seen that the groups of the adsorbent have not changed significantly, indicating that the prepared adsorbent has excellent stability in the process of degrading tetracycline residual pollutants.
[0142] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing an adsorbent material for treating antibiotics in wastewater, characterized in that: The following steps are involved: Copper phenylacetylene and nano-perylene imide are dispersed in an organic solvent, and then a hydrothermal reaction is carried out at 80°C to 220°C to obtain a copper phenylacetylene / perylene imide composite material. The copper phenylacetylene / perylene imide composite material is used as an adsorption material for treating antibiotics in wastewater.
2. The preparation method according to claim 1, characterized in that The mass ratio of the copper phenylacetylene to the nano-perylene imide is 1:0.1-10.
3. The preparation method according to claim 1, characterized in that: The organic solvent is one or more of an alcohol solvent and N,N-dimethylformamide.
4. The preparation method according to claim 1, characterized in that: The usage ratio of the organic solvent to the copper phenylacetylene is 10 mL to 100 mL: 15 mg to 120 mg.
5. The preparation method according to claim 1, characterized in that: The copper phenylacetylene and nano-perylene imide are dispersed in an organic solvent by first stirring and then ultrasonic treatment.
6. The preparation method according to claim 5, characterized in that: The ultrasonic treatment time is 2 min to 100 min.
7. The preparation method according to claim 5, characterized in that: The stirring time is 20 min to 180 min.
8. The preparation method according to claim 1, characterized in that: The hydrothermal reaction time is 1 h to 16 h.
9. An adsorbent material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the adsorption material according to claim 9 in adsorbing antibiotics in wastewater.
Citation Information
Patent Citations
Novel cuprous oxide and copper phenylacetylene compounded organic wastewater adsorbent
CN114682226A
Cited By
Preparation method and application of monatomic cocatalyst
CN122582960A