Method for preventing thickness unevenness of two shoulders of aircraft tire
By pre-setting the tire blank and superheated water treatment in the vulcanized capsule during the manufacturing process of aviation tires, combined with the chuck fixing technology, the problem of uneven thickness on both shoulders of the tire is solved, the balance performance and service life of the tire are improved, and the balance performance and service life of the tire are reduced. production costs.
Patent Information
- Application Number
- CN202411383961.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
During the manufacturing process of aviation tires, uneven thickness of the two shoulders of the vulcanized tires leads to poor balance performance, shortening service life, and increasing replacement frequency and cost.
Pre-shaped tire blanks under pressurized conditions. After setting, superheated water is injected into the vulcanized capsules to increase the shaping pressure and shorten the pressure holding time. Use a chuck to fix the vulcanized capsules to prevent loosening, and optimize the vulcanization process to reduce the The fluid flow is uneven.
Effectively prevent uneven thickness of both shoulders of aviation tires, improve the quality of finished products and production pass rate, extend the service life of tires, and reduce costs.
Smart Images

Figure CN119078254A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aviation tire manufacturing, and in particular relates to a method for preventing uneven thickness of two shoulders of an aviation tire. Background Art
[0002] With the growing demand for aircraft tires in China, it is urgent to solve the quality problems that arise in the manufacturing process of aircraft tires. At present, the uneven thickness of the two shoulders of the tire after vulcanization will affect the balance performance of the tire and shorten the service life of the tire.
[0003] According to the actual production situation, the reasons for the uneven thickness of the two shoulders of the tire are: 1. The semi-finished parts of the tire, such as tread rubber, cord layer, carcass transition film, etc., have poor size uniformity when extruded; 2. During the molding process of the tire, the semi-components such as the left and right cords of the machine head are not subjected to the same force, and the center line of the semi-components is not centered with the center line of the cursor of the machine head, so the symmetry of the tire during the molding process cannot be guaranteed; 3. During the vulcanization and shaping of the tire, the carcass is under the action of the bladder expansion tension and the carcass cord tension, and the rubber material on the upper and lower sides of the carcass flows unevenly. After strictly controlling the extrusion size of the molded semi-components and the molding operation of the tire, the problem of uneven thickness of the two shoulders of the tire has been alleviated to a certain extent. However, in actual applications, when the semi-components are uniform in size and a bladder reverse packaging molding machine with high precision and uniform force on the positive and reverse packages is used, some tires still have the problem of uneven thickness of the two shoulders.
[0004] After analysis, it is found that the larger the cross-sectional width and outer diameter of the aircraft tire, the larger the volume of the cavity, and the more likely it is to have quality problems such as uneven thickness of the two shoulders after vulcanization. Due to the characteristics of the specifications of such large-sized tires, the volume of the tire cavity is large, and the area where the bladder and the tire itself are stretched is large, so the vulcanization shaping process is difficult to control and the process stability is poor. When the bladder expands unevenly from top to bottom and the tire stretches unevenly inside, the flow speed of the rubber material is inconsistent. Under the action of high temperature and high pressure, the outer contour of the tire has uneven thickness of the two shoulders due to inconsistent material distribution on the upper and lower sides of the model.
[0005] When the problem of uneven thickness on the two shoulders of an aviation tire is serious, the balance difference value of the finished tire will increase. Tires with uneven thickness on the two shoulders will have uneven friction during takeoff and landing, which will destroy the stability of the tire use, and are more likely to cause increased tire wear, shorten tire service life, and increase the frequency and cost of tire replacement. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preventing uneven thickness of two shoulders of an aircraft tire. The method provided by the present invention can prevent uneven thickness of two shoulders of an aircraft tire, improve the quality of finished aircraft tires and the production qualification rate, thereby extending the service life of the tire and reducing costs.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preventing uneven thickness of two shoulders of an aircraft tire, comprising the following steps:
[0009] Pre-shaping the green tire under pressure to obtain a pre-shaped green tire;
[0010] Putting the pre-shaped tire into a vulcanizing bladder for shaping, and obtaining a shaped tire in the vulcanizing bladder, wherein the shaping pressure is ≥ 0.18 MPa and the pressure holding time is < 30 s;
[0011] Superheated water is injected into the vulcanizing bladder, and the pressure of the superheated water is ≥1.75 MPa; then the shaped tire blank is subjected to positive vulcanization to obtain an aviation tire.
[0012] Preferably, before the shaping, the method further comprises: fixing the vulcanizing bladder with a chuck, the chuck comprising a pressure plate and a tray, the pressure plate and the tray being fixedly connected with bolts, the bolts being sleeved with spring washers, and the spring washers being arranged between the nuts of the bolts and the pressure plate.
[0013] Preferably, the predetermined forming pressure is 0.3-0.4 MPa.
[0014] Preferably, the height of the predetermined tire blank is 100 to 250 mm less than the height of the tire blank.
[0015] Preferably, the shaping pressure is 0.18-0.2 MPa.
[0016] Preferably, the holding time for shaping is 20 to 25 seconds.
[0017] Preferably, the pressure of the superheated water is 1.75-2.5 MPa.
[0018] Preferably, the superheated water is injected into the vulcanizing bladder for 1 to 3 minutes.
[0019] Preferably, the number of cord plies of the aircraft tire is ≥16.
[0020] Preferably, the size of the aircraft tire is ≥ 21 inches.
[0021] The present invention provides a method for preventing uneven thickness of two shoulders of an aircraft tire, comprising the following steps: pre-forming a tire blank under pressure to obtain a pre-formed tire blank; placing the pre-formed tire blank into a vulcanization bladder for shaping to obtain a shaped tire blank in the vulcanization bladder, wherein the shaping pressure is ≥0.18MPa and the pressure holding time is <30s; injecting superheated water into the vulcanization bladder, wherein the pressure of the superheated water is ≥1.75MPa; and then vulcanizing the shaped tire blank to obtain an aircraft tire. Before shaping the tire blank, the present invention pre-forms the tire blank under pressure, reduces the height of the tire blank by pre-forming, and ensures that the tire blank maintains a stable profile during the subsequent positive vulcanization process. At the same time, the present invention increases the shaping pressure and shortens the shaping holding time. When the tire blank has been pre-shaped, increasing the shaping pressure can enable the tire blank to quickly reach an ideal shaping profile and improve the stability of the tire blank under stress and stretching; after the shaping profile of the tire blank is stable, the shaping holding time is shortened to keep the tire blank in a stable profile state for positive vulcanization. Finally, the present invention increases the pressure of the hot water after shaping and before vulcanization, thereby reducing the unevenness of the flow of the rubber material of the tire blank in the vulcanization bladder model. In summary, the present invention prevents uneven thickness of the two shoulders of the aircraft tire through reasonable optimization of pre-shaping, shaping and hot water steps and parameters, improves the quality of the finished aircraft tire and the production qualification rate, thereby extending the service life of the tire and reducing costs.
[0022] Furthermore, in the present invention, before the shaping, the method further includes: fixing the vulcanizing bladder with a chuck, the chuck including a pressure plate and a tray, the pressure plate and the tray being fixedly connected with bolts, the bolts being covered with spring washers, the spring washers being arranged between the nuts of the bolts and the pressure plate. The present invention adds a spring washer (such as Figure 1 As shown), the vulcanization bladder is prevented from loosening during use, and local deformation of the vulcanization bladder is avoided, and uneven stretching occurs after expansion. If uneven stretching occurs during the process of shaping and vulcanization of the vulcanization bladder, the center line of the vulcanization bladder will deviate, and continuing to use the vulcanization bladder in this situation will aggravate the problem of uneven thickness of the tire shoulder. The present invention can prevent the vulcanization bladder from loosening by adding a spring washer, and make the outer edge of the vulcanization bladder evenly stressed, avoid irregular deformation of the height of the vulcanization bladder clamping edge, balance the overall compression of the vulcanization bladder, not only extend the service life of the vulcanization bladder, but also prevent uneven thickness of the two shoulders of the aircraft tire, improve the quality of the finished aircraft tire and the production qualification rate, thereby extending the service life of the tire and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the assembly diagram of the curing bladder chuck;
[0024] Figure 1Middle: 1 is capsule, 2 is upper tray, 3 is upper pressing plate, 4 is spring washer, 5 is screw;
[0025] Figure 2 Schematic diagram of the thickness of the tire shoulder in an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a method for preventing uneven thickness of two shoulders of an aircraft tire, comprising the following steps:
[0027] Pre-shaping the green tire under pressure to obtain a pre-shaped green tire;
[0028] Putting the pre-shaped tire into a vulcanizing bladder for shaping, and obtaining a shaped tire in the vulcanizing bladder, wherein the shaping pressure is ≥ 0.18 MPa and the pressure holding time is < 30 s;
[0029] Superheated water is injected into the vulcanizing bladder, and the pressure of the superheated water is ≥1.75 MPa; then the shaped tire blank is subjected to positive vulcanization to obtain an aviation tire.
[0030] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0031] The present invention pre-shapes the tire blank under pressure to obtain a pre-shaped tire blank. In the present invention, the present invention has no special requirements for the preparation method of the tire blank, and a preparation method well known to those skilled in the art can be used. In the present invention, the tire blank is a tire blank with uniform semi-components and good molding quality. The pre-shaping is performed using a shaping machine. The pre-shaping pressure is preferably 0.3 to 0.4 MPa. The height of the pre-shaped tire blank is preferably 100 to 250 mm less than the height of the tire blank, and more preferably 150 to 210 mm.
[0032] After obtaining the predetermined tire blank, the present invention places the predetermined tire blank into a vulcanization bladder for shaping, and obtains a shaped tire blank in the vulcanization bladder, wherein the shaping pressure is ≥0.18MPa, and the pressure holding time is <30s. In the present invention, before the shaping, the present invention preferably further comprises: fixing the vulcanization bladder with a chuck, wherein the chuck comprises a pressure plate and a tray, wherein the pressure plate and the tray are fixedly connected with bolts, wherein a spring washer is sleeved on the bolt, and wherein the spring washer is arranged between the nut of the bolt and the pressure plate.
[0033] In the present invention, the shaping pressure is preferably 0.18-0.2MPa; the shaping holding time is preferably 20-25s, more preferably 20s. The present invention optimizes the shaping pressure to 0.18-0.2MPa, and optimizes the shaping holding time to 20-25s. When the green tire has been pre-shaped, the green tire can quickly reach the ideal shaping contour and improve the stability of the green tire under stress and stretching; after the green tire shaping contour is stable, the holding time is 20-25s, which can keep the green tire contour stable for positive vulcanization.
[0034] After obtaining the shaped tire blank, the present invention injects superheated water into the vulcanization bladder, and the pressure of the superheated water is ≥1.75MPa; then the shaped tire blank is subjected to positive vulcanization to obtain an aircraft tire. In the present invention, the pressure of the superheated water is ≥1.75MPa, preferably 1.75-2.5MPa. The time for injecting superheated water into the vulcanization bladder is preferably 1-3min. In the prior art, the pressure of the hot water before positive vulcanization is 1.5-2.0MPa. The present invention increases the pressure of the hot water to 1.75-2.5MPa, that is, the present invention increases the pressure of the hot water by 0.25-0.5MPa. The present invention optimizes and increases the pressure of the hot water before positive vulcanization after shaping, and shortens the time of injecting superheated water. For large-sized tires with a large number of carcass cord layers, the present invention increases the pressure of the hot water injected into the vulcanization bladder before positive vulcanization and shortens the time of injecting the internal pressure, while keeping the external temperature rising condition unchanged, which can reduce the unevenness of the flow of the rubber in the vulcanization bladder model.
[0035] In the present invention, the temperature of the vulcanization is preferably 135-140° C., specifically 138° C. The time of the vulcanization is preferably 80-100 min, specifically 90 min. The pressure of the superheated water during the vulcanization is preferably 2.5-3.1 MPa.
[0036] In the present invention, the aircraft tire is a large-size aircraft tire, and the number of plies of the aircraft tire is preferably ≥ 16. The size of the aircraft tire is preferably ≥ 21 inches.
[0037] In an embodiment of the present invention, the number of plies of the aircraft tire is 16. The size of the aircraft tire is 21 inches.
[0038] In summary, the present invention provides a method for preventing uneven thickness of upper and lower shoulders of large-sized aircraft tires (with ≥16 plies and ≥21 inches in size). The present invention solves the problem of uneven thickness of the shoulders of large-sized aircraft tires by: pre-forming the tire blank; adding a spring washer for fixing the screw rod with a chuck; appropriately increasing the shaping pressure and shortening the shaping holding time; increasing the pressure of the hot water before vulcanization after shaping and shortening the hot water time before vulcanization; and improving the tire production quality and product qualification rate.
[0039] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0040] Example 1
[0041] 200 21-inch aviation bias tires with 16 carcass plies were divided into groups for control tests. 200 green tires with uniform semi-components and good molding quality were divided into 4 groups for verification tests: Group 1: 20 green tires were prepared using the method 1 scheme; Group 2: 20 green tires were prepared using the method 2 scheme; Group 3: 20 green tires were prepared using the methods 3 and 4 schemes; Group 4: 120 green tires were prepared using the methods 1, 2, 3 and 4 schemes. Control group: The remaining 20 green tires were prepared using conventional methods.
[0042] Method 1 of the first group is: pre-forming the tire blank with a shaping machine, adjusting the wind pressure of the shaping machine to 0.4MPa for pre-forming, reducing the height of the tire blank from 810mm to 600mm after pre-forming, and obtaining a pre-shaped tire blank; placing the pre-shaped tire blank into a vulcanizing bladder for shaping, fixing the vulcanizing bladder before shaping, the vulcanizing bladder is fixed by a chuck, the chuck includes a pressure plate and a tray, the pressure plate and the tray are provided with bolt holes, the pressure plate and the tray are fixedly connected by bolts, and no spring washer is provided between the nut of the bolt and the pressure plate. The shaping pressure is 0.13-0.15MPa, and the shaping holding time is 30s. Then, the shaped tire blank is vulcanized in a vulcanizing bladder. Before the vulcanization, hot water is injected into the vulcanizing bladder at a pressure of 1.6 to 1.8 MPa for 5 minutes. Then, the aircraft tire is obtained after vulcanization under the vulcanization conditions of an external temperature of 138° C., a time of 90 minutes, and a superheated water pressure of 2.5 to 3.1 MPa.
[0043] The second group's method 2 is as follows: the tire blank is placed in a vulcanization bladder for shaping, the vulcanization bladder is fixed before shaping, the vulcanization bladder is fixed by a chuck, the chuck includes a pressure plate and a tray, the pressure plate and the tray are provided with bolt holes, the pressure plate and the tray are fixedly connected by bolts, a spring washer is sleeved on the bolt, and the spring washer is arranged between the nut of the bolt and the pressure plate. The shaping pressure is 0.13-0.15MPa, and the shaping holding time is 30s. Then, the shaped tire blank is vulcanized in the vulcanization bladder, and hot water is injected into the vulcanization bladder before vulcanization, the pressure is 1.6-1.8MPa, and the time of injecting hot water is 5min, and then the aircraft tire is obtained after vulcanization according to the positive vulcanization conditions of external temperature 138℃, time 90min, and superheated water pressure of 2.5-3.1MPa.
[0044] The schemes of method 3 and method 4 of the third group are as follows: the tire blank is placed in a vulcanization bladder for shaping, the vulcanization bladder is fixed before shaping, the vulcanization bladder is fixed by a chuck, the chuck includes a pressure plate and a tray, the pressure plate and the tray are provided with bolt holes, the pressure plate and the tray are fixedly connected by bolts, and no spring washer is provided between the nut of the bolt and the pressure plate. The shaping pressure is 0.18-0.20MPa, and the shaping holding time is 20s. Then the shaped tire blank is vulcanized in the vulcanization bladder, and hot water is injected into the vulcanization bladder before vulcanization, the pressure is 1.75-2.0MPa, and the time of injecting hot water is 1-3min, and then the aircraft tire is obtained after vulcanization according to the positive vulcanization conditions of external temperature 138℃, time 90min, and superheated water pressure of 2.5-3.1MPa.
[0045] The schemes of method 1, method 2, method 3 and method 4 of the fourth group are as follows: pre-forming the tire blank with a shaping machine, adjusting the wind pressure of the shaping machine to 0.4MPa for pre-forming, reducing the height of the tire blank from 810mm to 600mm after pre-forming, and obtaining a pre-shaped tire blank; placing the pre-shaped tire blank into a vulcanizing bladder for shaping, fixing the vulcanizing bladder before shaping, the vulcanizing bladder is fixed by a chuck, the chuck includes a pressure plate and a tray, the pressure plate and the tray are provided with bolt holes, the pressure plate and the tray are fixedly connected by bolts, a spring washer is sleeved on the bolt, and the spring washer is provided between the nut of the bolt and the pressure plate. The shaping pressure is 0.18-0.20MPa, and the shaping holding time is 20s. Then, the shaped tire blank is vulcanized in a vulcanizing bladder. Before the vulcanization, hot water is injected into the vulcanizing bladder at a pressure of 1.75 to 2.0 MPa for 1 to 3 minutes. Then, the aircraft tire is vulcanized according to the vulcanization conditions of an external temperature of 138° C., a time of 90 minutes, and a superheated water pressure of 2.5 to 3.1 MPa.
[0046] The conventional method of the control group is: the tire blank is placed in a vulcanization bladder for shaping, the vulcanization bladder is fixed before shaping, the vulcanization bladder is fixed by a chuck, the chuck includes a pressure plate and a tray, the pressure plate and the tray are provided with bolt holes, the pressure plate and the tray are fixedly connected by bolts, and no spring washer is provided between the nut of the bolt and the pressure plate. The shaping pressure is 0.13-0.15MPa, and the shaping holding time is 30s. Then, the shaped tire blank is vulcanized in the vulcanization bladder, and hot water is injected into the vulcanization bladder before vulcanization, the pressure is 1.6-1.8MPa, and the time of injecting hot water is 5min, and then the aircraft tire is obtained after vulcanization according to the positive vulcanization conditions of external temperature 138℃, time 90min, and superheated water pressure of 2.5-3.1MPa.
[0047] After vulcanization, the difference in average thickness of the two shoulders of the batch of tires is measured using a non-destructive tire rubber thickness gauge (hereinafter referred to as Surfix rubber thickness gauge). The Surfix rubber thickness gauge uses the principle of electromagnetic induction. Without destroying the tire, the rubber material in each part has different magnetic changes, so as to calculate the thickness of different base layers.
[0048] The thickness of the two shoulders of each trial-produced tire was measured using the Surfix rubber thickness gauge. The difference in average thickness of the two shoulders of each set of tires is shown in Table 1:
[0049] Table 1 Results of the difference in average thickness of the two shoulders of five groups of tires produced
[0050]
[0051] From the results in Table 1, we know that the methods of the first, second, third and fourth groups all play a certain role in preventing the uneven thickness of the shoulders of large-sized aircraft tires. The method of pre-molding the blank of the first group is more effective than the methods of the second and third groups, but the method of the fourth group is the best. The average thickness difference of the shoulders of the aircraft tires prepared by the fourth group method is reduced from 7.6mm in the control group to 2.25mm, which is within the acceptable range of process control. The shoulder thickness of the fourth group of trial tires is as follows: Figure 2 As shown, the shoulder thickness measurement position is Figure 2 The white line in the middle.
[0052] It can be seen from the above embodiments that the present invention provides a method for preventing uneven thickness of upper and lower shoulders of large-sized aircraft tires (with 16 plies and a size of 21 inches). The present invention adopts the following methods: pre-forming the tire blank (the pre-forming pressure is 0.3-0.4 MPa); adding spring washers for fixing the chuck bolts; appropriately increasing the shaping pressure (the shaping pressure is 0.18-0.2 MPa), shortening the shaping holding time (the shaping holding time is 20-25 s); increasing the hot water pressure before vulcanization after shaping (the pressure is 1.75-2.5 MPa), and shortening the hot water time before vulcanization (1-3 min); solving the problem of uneven thickness of the shoulders of large-sized aircraft tires, improving tire production quality, and improving product qualification rate.
[0053] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preventing uneven thickness of two shoulders of an aircraft tire, characterized in that: The following steps are involved: Pre-shaping the green tire under pressure to obtain a pre-shaped green tire; Putting the pre-shaped tire into a vulcanizing bladder for shaping, and obtaining a shaped tire in the vulcanizing bladder, wherein the shaping pressure is ≥ 0.18 MPa and the pressure holding time is < 30 s; Superheated water is injected into the vulcanizing bladder, and the pressure of the superheated water is ≥1.75 MPa; then the shaped tire blank is subjected to positive vulcanization to obtain an aircraft tire.
2. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1, characterized in that: Before the shaping, the method further includes: fixing the vulcanizing bladder with a chuck, wherein the chuck includes a pressure plate and a tray, the pressure plate and the tray are fixedly connected with bolts, a spring washer is sleeved on the bolt, and the spring washer is arranged between the nut of the bolt and the pressure plate.
3. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1, characterized in that: The predetermined forming pressure is 0.3-0.4 MPa.
4. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1 or 3, characterized in that: The height of the predetermined tire blank is 100 to 250 mm less than the height of the tire blank.
5. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1, characterized in that: The shaping pressure is 0.18-0.2 MPa.
6. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1 or 5, characterized in that: The holding time for the shaping is 20 to 25 seconds.
7. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1, characterized in that: The pressure of the superheated water is 1.75-2.5 MPa.
8. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1 or 7, characterized in that: The time for injecting superheated water into the vulcanizing bladder is 1 to 3 minutes.
9. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1, characterized in that: The number of ply layers of the aircraft tire is ≥16.
10. The method for preventing uneven thickness of two shoulders of an aircraft tire according to claim 1 or 9, characterized in that: The size of the aircraft tire is ≥ 21 inches.