Hydraulic asphalt and preparation method thereof
Through a process without polymer modification, combining single cycloalkyl crude oil and oil sand asphalt, and using polyphosphoric acid and dodecyl benzene sulfonic acid modifiers, polymer degradation and polymer degradation in hydraulic asphalt production are solved and The complex construction problem has achieved high-temperature aging resistance and low-temperature delay hydroassine products, meeting the strict performance requirements of water conservancy projects.
Patent Information
- Application Number
- CN202310652549.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
The existing hydraulic asphalt production process has problems such as polymer degradation, complex construction and high production costs, which are difficult to meet the strict requirements of water conservancy projects for high-temperature aging resistance and low-temperature brittle crack resistance.
Using a polymer-free modification process, No. 70 A grade asphalt refined through a single cycloalkyl crude oil is combined with oil sand asphalt, polyphosphoric acid and dodecylbenzenesulfonic acid are added as modifiers, and the Hydrotherapy and decompression deep extraction are prepared by hydrotreating and optimizing its structure and performance.
It has achieved the improvement of high-temperature performance, low-temperature delay and anti-aging properties of hydraulic asphalt, meets the technical requirements of the No. 2 hydraulic asphalt in the "hydraulic petroleum asphalt" product standard SH/T0799-2007, and expands the use of inferior raw materials and Reduced production costs.
Smart Images

Figure BDA0004265622280000051 
Figure BDA0004265622280000061 
Figure BDA0004265622280000062
Abstract
Description
Technical Field
[0001] The invention relates to the fields of water conservancy and petrochemical engineering, and in particular to hydraulic asphalt and a preparation method thereof. Background Art
[0002] As a special asphalt material among petroleum asphalt, hydraulic asphalt has excellent flexibility and anti-seepage properties. It is widely used in the construction of water conservancy projects such as reservoirs, earth-rock dams, canal embankments and channel anti-seepage.
[0003] Compared with conventional reinforced concrete, hydraulic asphalt concrete is a viscoelastic-plastic material. Its main characteristics are its advantages in adaptability to deformation and anti-seepage performance. In addition, hydraulic asphalt concrete also has the advantages of small engineering volume and fast construction. With the rapid development of China's hydropower industry and the advancement of asphalt concrete anti-seepage technology, more and more water conservancy projects will adopt asphalt concrete anti-seepage technology. Since hydraulic asphalt is an important raw material for asphalt concrete anti-seepage, in order to ensure the safety and durability of water conservancy projects, very strict quality requirements are put forward for hydraulic asphalt, requiring good high temperature aging resistance and low temperature brittle crack resistance.
[0004] In 2008, China began to implement the petrochemical industry standard "Hydraulic Petroleum Asphalt" product standard SH / T0799-2007. Among them, different grades of hydraulic asphalt quality index requirements are proposed for different hydraulic asphalt concrete construction structures. Among them, No. 1 hydraulic asphalt is mainly suitable for the anti-seepage layer of hydraulic structure panels, No. 2 hydraulic asphalt is mainly suitable for the core wall of hydraulic structure, and No. 3 hydraulic asphalt is mainly suitable for the sealing layer of hydraulic structure. At present, most of the production of hydraulic asphalt adopts SBS modified production process. Although the technology is feasible from the perspective of hydraulic asphalt technical indicators, the degradation of polymers may reduce the service life of hydraulic asphalt. Therefore, the existing hydraulic asphalt development technology needs to be further improved, which is also of great significance to the development of water conservancy engineering.
[0005] CN100365098C discloses a method for preparing hydraulic asphalt. The method uses a mild oxidation process, selects basic raw materials with suitable properties such as consistency (i.e., needle penetration value) and density, and suitable process conditions, and introduces oxygen or oxygen-containing gas (such as air) into the heated and molten basic asphalt for moderate oxidation to prepare a hydraulic asphalt product. The oxidation process will produce a large amount of waste gas, pollute the environment, and the subsequent treatment is relatively complicated. At present, this process is rarely used to produce hydraulic asphalt.
[0006] CN114479494A discloses a hydraulic asphalt with excellent adhesion and a preparation method thereof. The modified asphalt comprises the following components by weight: 100 parts of 70# base asphalt; 1.5-3.8 parts of SBS modifier; 0-1.5 parts of SBR modifier; 1.3-3.8 parts of retardant; 0.5-1 parts of anti-stripping agent; 0.08-0.2 parts of stabilizer. The hydraulic modified asphalt has many problems such as polymer service life, production and construction difficulties, and high modification cost, which limits the large-scale use of this process.
[0007] CN103232712B discloses a hydraulic asphalt and a preparation method thereof. The method obtains a hydraulic asphalt product that meets the index requirements by performing SBS / waste rubber powder composite modification on heavy traffic asphalt. Although the hydraulic asphalt has good low-temperature crack resistance, the preparation process is complicated, the production cost is high, and the SBS modifier and waste rubber powder modifier used have poor stability, which affects the service life of the project. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a hydraulic asphalt and a preparation method thereof. The various indicators of the hydraulic asphalt meet the technical requirements for No. 2 hydraulic asphalt in the "hydraulic petroleum asphalt" product standard SH / T0799-2007.
[0009] The first aspect of the present invention provides a hydraulic asphalt, which comprises the following raw material components in parts by weight:
[0010] First matrix asphalt: 100 parts;
[0011] Performance regulator: 8 to 25 parts, preferably 10 to 20 parts;
[0012] Pretreatment agent: 3 to 12 parts, preferably 5 to 10 parts;
[0013] The performance regulator comprises the following raw material components by weight:
[0014] Second base asphalt: 100 parts;
[0015] Oil sand asphalt: 20-60 parts, preferably 30-50 parts;
[0016] Modifier: 0.1 to 2 parts, preferably 0.2 to 1.2 parts.
[0017] The hydraulic asphalt does not contain high molecular polymers, such as SBS, SBR and other high molecular polymers.
[0018] The first matrix asphalt is a No. 70A grade asphalt refined from a single cycloalkyl crude oil, and its basic properties meet the "road petroleum asphalt technology" index requirements of the corresponding grade.
[0019] The second base asphalt is a 70#A grade asphalt refined from a single naphthenic crude oil, and its basic properties meet the "road petroleum asphalt technology" index requirements of the corresponding grade. The properties of the second base asphalt and the first base asphalt can be completely the same or different, and their basic properties can meet the "road petroleum asphalt technology" index requirements of the corresponding grade.
[0020] The oil sands asphalt is one or more of Inner Mongolia oil sands asphalt, Qinghai oil sands asphalt, Indonesian oil sands asphalt, and Kazakhstan oil sands asphalt.
[0021] The properties of the oil sand asphalt include: a softening point of not less than 50°C, preferably 55°C to 65°C, a flash point of not less than 232°C, preferably 235°C to 256°C, a solidification point of 25°C to 32°C, and a viscosity of 1450 to 1600 mm at 100°C. 2 / s, preferably 1500~1600mm 2 / s, the residual carbon is 9.5wt% ~ 15.1wt%, the sulfur content is 2.0wt% ~ 6.1wt%, the carbon content is 84wt% ~ 87wt%, the hydrogen content is 10wt% ~ 12.4wt%, the nitrogen content is 0.2wt% ~ 0.8wt%, and by mass fraction, the saturated component accounts for 10.1% ~ 30.7%, the aromatic component accounts for 15.6% ~ 35.9%, the gum accounts for 30.4% ~ 45.8%, the asphaltenes account for 10.7% ~ 27.3%, and the asphaltenes preferably account for 11.3% ~ 25.2%.
[0022] The modifier is a mixture of polyphosphoric acid and dodecylbenzene sulfonic acid, wherein the mass content of phosphoric acid contained in the polyphosphoric acid is 125% to 145% in terms of H3PO4, preferably 130% to 140%; the dodecylbenzene sulfonic acid can be C 18 H 30 Industrial grade dodecylbenzene sulfonic acid with SO3 content ≥96wt%.
[0023] In the mixture of polyphosphoric acid and dodecylbenzene sulfonic acid, the mass ratio of polyphosphoric acid to dodecylbenzene sulfonic acid is 1:3 to 1:5.
[0024] The pretreatment agent comprises the following raw material components by weight:
[0025] Third matrix asphalt: 100 parts;
[0026] Middle component: 20-60 parts, preferably 25-50 parts;
[0027] Light component: 5 to 35 parts, preferably 10 to 30 parts.
[0028] The third matrix asphalt is a No. 70 grade A asphalt refined from a single cycloalkyl crude oil, and its basic properties meet the "road petroleum asphalt technology" index requirements of the corresponding grade.
[0029] The properties of the third matrix asphalt can be completely the same as or different from those of the first matrix asphalt and the second matrix asphalt, as long as their basic properties meet the "road petroleum asphalt technology" index requirements of the corresponding brand.
[0030] The middle mass component refers to the colloid obtained after solvent deasphalting, and the middle mass component has the following properties: kinematic viscosity at 100°C is 50 mm 2 / s~65mm 2 / s, the flash point is 206℃~220℃, by mass fraction, the saturated fraction accounts for 30%~42%, the aromatic fraction accounts for 48%~57%, the gum accounts for 8%~13%, and the asphaltene content is less than 2%; the weight average molecular weight is 1990~2140, and the molecular weight distribution width is 1.6~3.7.
[0031] The light component refers to vacuum wax oil, and the light component has the following properties: 50°C kinematic viscosity is 10 mm 2 / s~16mm 2 / s, density at 20℃ is 760~900kg / m 3 , by mass fraction, the saturated content accounts for 60% to 78%, the aromatic content accounts for 20% to 32%, the total content of colloids and asphaltene is less than 6%; the residual carbon is less than 0.15wt%, the sulfur content is less than 0.3wt%, the nitrogen content is less than 1wt%, and the hydrogen-carbon molar ratio is 1.5 to 1.8.
[0032] The present invention also provides a method for preparing the above hydraulic asphalt, which comprises the following steps:
[0033] (1) preparing a performance modifier;
[0034] (2) preparing a pretreatment agent;
[0035] (3) The first matrix asphalt is blended with a performance regulator and a pretreatment agent to obtain the hydraulic asphalt.
[0036] The process of preparing the performance-adjusting agent in step (1) is as follows:
[0037] The second matrix asphalt heated to a fluid state, the oil sand asphalt and the modifier are added into a reactor, stirred and heated to the reaction temperature, and heat-insulated after the reaction is completed; after the heat-insulation is completed, vacuum deep drawing is performed to obtain a performance regulator.
[0038] The temperature at which the second matrix asphalt is heated to a fluid state is 140° C. to 155° C.
[0039] The reactor is a high-pressure reactor, and the initial temperature of the reactor is adjusted to 130° C. to 150° C.
[0040] The stirring speed is 600-800 r / min. The heating to the reaction temperature is carried out by programmed temperature increase, the heating rate is 1°C-3°C / min, the reaction temperature is 140°C-180°C, preferably 155°C-170°C; the reaction time is 3-6h.
[0041] The heat preservation treatment conditions are: heat preservation at 120° C. to 135° C. for 10 to 16 hours.
[0042] The termination temperature of the reduced pressure deep drawing is 495° C. to 520° C. (normal pressure temperature after conversion).
[0043] The process of preparing the pretreatment agent in step (2) is as follows:
[0044] i. After the third matrix asphalt heated to a fluid state is mixed with the medium component and the light component, hydrogen is added for hydrogenation treatment;
[0045] ii. The material obtained in step i is subjected to atmospheric and vacuum distillation to obtain the final pretreated component.
[0046] In step i, the operating conditions of the hydrotreatment are: reaction temperature of 365°C to 390°C, reaction pressure of 12MPa to 22MPa, volume space velocity of 0.5 to 1.8h -1 , hydrogen-to-oil volume ratio is 400-1500; the preferred operating conditions are: reaction temperature is 370°C-390°C, reaction pressure is 13MPa-20MPa, volume space velocity is 0.5-1.2h -1 , the volume ratio of hydrogen to oil is 500-1100.
[0047] In step i, the reactor used for the hydrotreatment can be at least one of a fixed bed hydrogenation reactor, an ebullated bed hydrogenation reactor or a suspended bed hydrogenation reactor, preferably an ebullated bed hydrogenation reactor.
[0048] In step i, the catalyst used for the hydroprocessing can be a commercially available catalyst, for example, the FF, FH, and FZC series catalysts developed by the Dalian Petrochemical Research Institute of Sinopec can be used. The catalyst grading method can be determined according to conventional methods and is not particularly limited in the present invention.
[0049] In step ii, the atmospheric and vacuum distillation is carried out in an atmospheric and vacuum distillation kettle. There are no special requirements for atmospheric distillation. The final temperature of the vacuum distillation is 465-540°C, preferably 485-520°C.
[0050] In step (3), the conditions for the blending treatment are: a temperature of 170 to 185° C., a blending stirring speed of 300 to 500 r / min, and a blending stirring time of 3 to 6 hours.
[0051] Compared with the prior art, the hydraulic asphalt and the preparation method thereof of the present invention have the following advantages:
[0052] (1) At present, since most of the production of hydraulic asphalt adopts high molecular polymer modification processes such as SBS, there are problems such as polymer degradation and complex construction. The present invention can meet the technical requirements of No. 2 hydraulic asphalt in the "Hydraulic Petroleum Asphalt" product standard SH / T0799-2007 without the help of any high molecular polymer modification.
[0053] (2) The oil sand asphalt used in the present invention is a low value-added raw material, which is not suitable for producing hydraulic asphalt by itself, such as the Inner Mongolia oil sand asphalt with high asphaltene content, very special existence form, and extremely inferior comprehensive performance. It cooperates with cycloalkyl asphalt, and after modification and vacuum deep drawing, the composition structure is optimized, the softening point and low-temperature ductility of the asphalt are improved, and the oil sand asphalt has high stability and can be used to prepare durable hydraulic asphalt, which expands the use of inferior raw materials and improves its added value.
[0054] (3) The present invention also introduces a pretreatment agent, which is obtained by hydrogenation treatment and secondary distillation of a third matrix asphalt, a medium component, and a light component. The treatment process adjusts and optimizes the average molecular structure, molecular weight distribution, etc. of the material, and the continuity of the material structure and composition is enhanced, so that the pretreatment component has the characteristics of low viscosity, high flash point, large low-temperature ductility, and low temperature sensitivity, which can make up for the shortcomings of directly preparing hydraulic asphalt from matrix asphalt. DETAILED DESCRIPTION
[0055] The technical solution of the present invention is further described below by way of examples, but these examples cannot limit the protection scope of the present invention, and the wt % involved is the mass fraction.
[0056] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent stores.
[0057] The base asphalt in the following examples and comparative examples all uses Qilu 70A asphalt, and the properties of the base asphalt and the technical index requirements of No. 2 hydraulic asphalt in the "Hydraulic Petroleum Asphalt" product standard SH / T0799-2007 are shown in Table 1. The properties of the oil sand asphalt, medium component, and light component used in the examples and comparative examples are shown in Tables 2 to 4.
[0058] Table 1 Properties of base asphalt and No. 2 hydraulic asphalt standards
[0059]
[0060]
[0061] Table 2 Properties of oil sand asphalt used in Examples and Comparative Examples
[0062] Carbon residue value / wt% 13.04 Carbon content / wt% 84.64 Nitrogen content / wt% 0.30 Hydrogen content / wt% 10.08 Sulfur content / wt% 2.64 Hydrogen-carbon molar ratio 1.42 Saturated fraction / wt% 11.38 Aromatic content / wt% 35.21 Gel / wt% 32.49 Asphaltene / wt% 20.92 Contraction Index CI 0.26 Ash / wt% 1.758 Mechanical impurities / wt% 2.59 Condensation point / ℃ 29.0 <![CDATA[Viscosity (100 °C) / mm 2 / s]]> 1553 Flash point / ℃ 238 Softening point / ℃ 57
[0063] Table 3 Properties of the intermediate components used in the examples and comparative examples
[0064]
[0065]
[0066] Table 4 Properties of the light components used in the examples and comparative examples
[0067] Saturated fraction / wt% 69.21 Aromatic content wt / % 26.36 Gel / wt% 4.32 Asphaltene / wt% 0.11 Carbon residue value / wt% 0.13 Sulfur content / wt% 0.24 Nitrogen content / wt% 0.18 Hydrogen-carbon molar ratio 1.8 <![CDATA[Kinematic viscosity at 50°C / mm 2 / s]]> 13 <![CDATA[Density at 20℃ / kg / m 3 > 817
[0068] Example 1
[0069] (1) 100 parts of the matrix asphalt (properties shown in Table 1) heated to a fluid state and 40 parts of the Inner Mongolia oil sand asphalt (properties shown in Table 2) were added to a high-pressure reactor at a temperature of 130°C and stirred, 0.2 parts of polyphosphoric acid with a phosphoric acid content (in terms of H3PO4) of 135% and 0.6 parts of dodecylbenzene sulfonic acid were slowly added to the reactor (added within 3 minutes), and the temperature was raised to 160°C at a rate of 2°C / min at a stirring speed of 600 r / min, and the reaction time was 4 hours; after the reaction was completed, the reactor was placed for insulation at a temperature of 120°C for 10 hours. After the insulation was completed, vacuum deep drawing was performed to obtain vacuum residue oil with a temperature greater than 500°C as a performance regulator.
[0070] (2) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 35 parts of the medium-weight component (partial properties shown in Table 3), and 20 parts of the light-weight component (partial properties shown in Table 4) were reacted at a reaction temperature of 380°C, a reaction pressure of 16 MPa, and a volume space velocity of 0.8 h -1 The hydrogenation treatment is carried out under the condition of hydrogen-to-oil volume ratio of 900. The hydrogenation catalyst is the FZC-301 catalyst developed by Sinopec Dalian Petrochemical Research Institute. The hydrogenation product is subjected to atmospheric and vacuum distillation. The distillation product above 500°C is the required pretreatment agent.
[0071] (3) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 15 parts of the performance regulator, and 8 parts of the pretreatment agent were stirred at 180° C. for 4.5 hours at a stirring speed of 400 r / min to obtain hydraulic asphalt A1.
[0072] Example 2
[0073] (1) 100 parts of the matrix asphalt (properties shown in Table 1) heated to a fluid state and 40 parts of the Inner Mongolia oil sand asphalt (properties shown in Table 2) were added to a high-pressure reactor at a temperature of 130°C and stirred, 0.3 parts of polyphosphoric acid with a phosphoric acid content (in terms of H3PO4) of 130% and 0.9 parts of dodecylbenzene sulfonic acid were slowly added to the reactor (added within 3 minutes), and the temperature was raised to 160°C at a rate of 2°C / min at a stirring speed of 600 r / min, and the reaction time was 4 hours; after the reaction was completed, the reactor was placed for insulation at a temperature of 120°C for 10 hours. After the insulation was completed, vacuum deep drawing was performed to obtain vacuum residue oil with a temperature greater than 510°C as a performance regulator.
[0074] (2) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 35 parts of the medium-weight component (partial properties shown in Table 3), and 20 parts of the light-weight component (partial properties shown in Table 4) were reacted at a reaction temperature of 380°C, a reaction pressure of 16 MPa, and a volume space velocity of 0.8 h -1 The hydrogenation treatment is carried out under the condition of hydrogen-to-oil volume ratio of 900. The hydrogenation catalyst is the FZC-301 catalyst developed by Sinopec Dalian Petrochemical Research Institute. The hydrogenation product is subjected to atmospheric and vacuum distillation. The distillation product above 500°C is the required pretreatment agent.
[0075] (3) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 15 parts of the performance regulator, and 6 parts of the pretreatment agent were stirred at 180° C. for 4.5 hours at a stirring speed of 400 r / min to obtain hydraulic asphalt A2.
[0076] Example 3
[0077] (1) 100 parts of the matrix asphalt (properties shown in Table 1) heated to a fluid state and 35 parts of the Inner Mongolia oil sand asphalt (properties shown in Table 2) were added to a high-pressure reactor at a temperature of 130°C and stirred, 0.1 parts of polyphosphoric acid with a phosphoric acid content (in terms of H3PO4) of 135% and 0.5 parts of dodecylbenzene sulfonic acid were slowly added to the reactor (added within 3 minutes), and the temperature was raised to 160°C at a rate of 2°C / min at a stirring speed of 600 r / min, and the reaction time was 4 hours; after the reaction was completed, the reactor was placed for insulation at a temperature of 120°C for 10 hours. After the insulation was completed, vacuum deep drawing was performed to obtain vacuum residue oil with a temperature greater than 500°C as a performance regulator.
[0078] (2) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 35 parts of the medium-weight component (partial properties shown in Table 3), and 20 parts of the light-weight component (partial properties shown in Table 4) were reacted at a reaction temperature of 380°C, a reaction pressure of 16 MPa, and a volume space velocity of 0.8 h -1The hydrogenation treatment is carried out under the condition of hydrogen-to-oil volume ratio of 900. The hydrogenation catalyst is the FZC-301 catalyst developed by Sinopec Dalian Petrochemical Research Institute. The hydrogenation product is subjected to atmospheric and vacuum distillation. The distillation product above 500°C is the required pretreatment agent.
[0079] (3) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 10 parts of the performance regulator, and 8 parts of the pretreatment agent were stirred at 180° C. for 5 h at a stirring speed of 400 r / min to obtain hydraulic asphalt A3.
[0080] Example 4
[0081] (1) 100 parts of the matrix asphalt (properties shown in Table 1) heated to a fluid state and 40 parts of the Inner Mongolia oil sand asphalt (properties shown in Table 2) were added to a high-pressure reactor at a temperature of 130°C and stirred, 0.2 parts of polyphosphoric acid with a phosphoric acid content (in terms of H3PO4) of 135% and 0.6 parts of dodecylbenzene sulfonic acid were slowly added to the reactor (added within 3 minutes), and the temperature was raised to 160°C at a rate of 2°C / min at a stirring speed of 600 r / min, and the reaction time was 4 hours; after the reaction was completed, the reactor was placed for insulation at a temperature of 120°C for 10 hours. After the insulation was completed, vacuum deep drawing was performed to obtain vacuum residue oil with a temperature greater than 500°C as a performance regulator.
[0082] (2) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 30 parts of the medium-weight component (partial properties shown in Table 3), and 25 parts of the light-weight component (partial properties shown in Table 4) were reacted at a reaction temperature of 380°C, a reaction pressure of 16 MPa, and a volume space velocity of 0.8 h -1 The hydrogenation treatment is carried out under the condition of hydrogen-to-oil volume ratio of 900. The hydrogenation catalyst is the FZC-301 catalyst developed by Sinopec Dalian Petrochemical Research Institute. The hydrogenation product is subjected to atmospheric and vacuum distillation. The distillation product above 495°C is the required pretreatment agent.
[0083] (3) 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 15 parts of the performance regulator, and 8 parts of the pretreatment agent were stirred at 180° C. for 4.5 hours at a stirring speed of 400 r / min to obtain hydraulic asphalt A4.
[0084] Comparative Example 1
[0085] The rest is the same as in Example 1, except that 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1), 35 parts of the medium-weight components (partial properties shown in Table 3), and 20 parts of the light-weight components (partial properties shown in Table 4) in step (2) are replaced with 155 parts of the base asphalt (properties shown in Table 1). Finally, hydraulic asphalt B1 is obtained.
[0086] Comparative Example 2
[0087] The rest is the same as Example 1, except that step (1) is omitted, and step (3) is performed by stirring 100 parts of the base asphalt (properties shown in Table 1) heated to a fluid state and 8 parts of the pretreatment agent at 180° C. for 4.5 hours at a stirring speed of 400 r / min. Finally, hydraulic asphalt B2 is obtained.
[0088] Comparative Example 3
[0089] The other parts are the same as in Example 1, except that the 100 parts of the base asphalt heated to a fluid state (properties shown in Table 1) and 40 parts of Inner Mongolia oil sand asphalt (properties shown in Table 2) in step (1) are replaced with 140 parts of Inner Mongolia oil sand asphalt (properties shown in Table 2). Finally, hydraulic asphalt B3 is obtained.
[0090] Test Case
[0091] Examples 1-4 and Comparative Examples 1-3 were analyzed and tested according to the technical index requirements of "Hydraulic Petroleum Asphalt" (SH / T0799-2007), and the results are shown in Table 5.
[0092] Table 5 Data table of hydraulic asphalt prepared in Examples 1-4 and Comparative Examples 1-3
[0093]
[0094] It can be seen from the results in Table 5 that the hydraulic asphalt prepared by the method of the present invention has excellent high temperature performance, low temperature ductility and anti-aging performance, and each performance can meet the technical index requirements of No. 2 hydraulic asphalt in the "Hydraulic Petroleum Asphalt" SH / T0799-2007 standard.
Claims
1. A hydraulic asphalt, characterized in that: By weight, it includes the following raw material components: First matrix asphalt: 100 parts; Performance regulator: 8 to 25 parts, preferably 10 to 20 parts; Pretreatment agent: 3 to 12 parts, preferably 5 to 10 parts; The performance regulator comprises the following raw material components by weight: Second base asphalt: 100 parts; Oil sand asphalt: 20-60 parts, preferably 30-50 parts; Modifier: 0.1 to 2 parts, preferably 0.2 to 1.2 parts.
2. The hydraulic asphalt according to claim 1, characterized in that: The first base asphalt is a No. 70A grade asphalt refined from a single naphthenic crude oil; and / or the second base asphalt is a No. 70A grade asphalt refined from a single naphthenic crude oil.
3. The hydraulic asphalt according to claim 1, characterized in that: The oil sands asphalt is one or more of Inner Mongolia oil sands asphalt, Qinghai oil sands asphalt, Indonesian oil sands asphalt, and Kazakhstan oil sands asphalt.
4. The hydraulic asphalt according to claim 1 or 3, characterized in that: The properties of the oil sand asphalt include: a softening point of not less than 50°C, preferably 55°C to 65°C, a flash point of not less than 232°C, preferably 235°C to 256°C, a solidification point of 25°C to 32°C, and a viscosity of 1450 to 1600 mm at 100°C. 2 / s, preferably 1500~1600mm 2 / s, the residual carbon is 9.5wt% ~ 15.1wt%, the sulfur content is 2.0wt% ~ 6.1wt%, the carbon content is 84wt% ~ 87wt%, the hydrogen content is 10wt% ~ 12.4wt%, the nitrogen content is 0.2wt% ~ 0.8wt%, and by mass fraction, the saturated component accounts for 10.1% ~ 30.7%, the aromatic component accounts for 15.6% ~ 35.9%, the gum accounts for 30.4% ~ 45.8%, the asphaltenes account for 10.7% ~ 27.3%, and the asphaltenes preferably account for 11.3% ~ 25.2%.
5. The hydraulic asphalt according to claim 1, characterized in that: The modifier is a mixture of polyphosphoric acid and dodecylbenzene sulfonic acid, wherein the mass ratio of the polyphosphoric acid to the dodecylbenzene sulfonic acid is 1:3 to 1:
5.
6. The hydraulic asphalt according to claim 1, characterized in that: The pretreatment agent comprises the following raw material components by weight: Third matrix asphalt: 100 parts; Middle component: 20-60 parts, preferably 25-50 parts; Light component: 5 to 35 parts, preferably 10 to 30 parts.
7. The hydraulic asphalt according to claim 6, characterized in that: The third matrix asphalt is No. 70 Grade A asphalt refined from single naphthenic crude oil.
8. The hydraulic asphalt according to claim 6, characterized in that: The middle mass component refers to the colloid obtained after solvent deasphalting, and the middle mass component has the following properties: kinematic viscosity at 100°C is 50 mm 2 / s~65mm 2 / s, the flash point is 206℃~220℃, by mass fraction, the saturated fraction accounts for 30%~42%, the aromatic fraction accounts for 48%~57%, the gum accounts for 8%~13%, and the asphaltene content is less than 2%; the weight average molecular weight is 1990~2140, and the molecular weight distribution width is 1.6~3.
7.
9. The hydraulic asphalt according to claim 6, characterized in that: The light component refers to vacuum wax oil, and the light component has the following properties: 50°C kinematic viscosity is 10 mm 2 / s~16mm 2 / s, density at 20℃ is 760~900kg / m 3 , by mass fraction, the saturated content accounts for 60% to 78%, the aromatic content accounts for 20% to 32%, the total content of colloids and asphaltene is less than 6%; the residual carbon is less than 0.15wt%, the sulfur content is less than 0.3wt%, the nitrogen content is less than 1wt%, and the hydrogen-carbon molar ratio is 1.5 to 1.
8.
10. The method for preparing hydraulic asphalt according to any one of claims 1 to 9, characterized in that: include: (1) preparing a performance modifier; (2) preparing a pretreatment agent; (3) The first matrix asphalt is blended with a performance regulator and a pretreatment agent to obtain the hydraulic asphalt.
11. The preparation method according to claim 10, characterized in that: The process of preparing the performance-adjusting agent in step (1) is as follows: Add the second matrix asphalt heated to a fluid state, the oil sand asphalt and the modifier into the reactor, stir and heat to the reaction temperature, and keep the temperature after the reaction is completed; After the heat preservation is completed, the vacuum deep drawing is carried out to obtain the performance regulator.
12. The preparation method according to claim 11, characterized in that: The temperature at which the second matrix asphalt is heated to a fluid state is 140°C to 155°C; the initial temperature of the reactor is adjusted to 130°C to 150°C; the stirring speed is 600 to 800 r / min; the heating to the reaction temperature is performed by programmed heating, and the heating rate is 1°C to 3°C / min, the reaction temperature is 140°C to 180°C, preferably 155°C to 170°C; the reaction time is 3 to 6 hours; the insulation treatment conditions are: insulation at 120°C to 135°C for 10 to 16 hours; the termination temperature of the reduced pressure deep drawing is 495°C to 520°C.
13. The preparation method according to claim 10, characterized in that: The process of preparing the pretreatment agent in step (2) is as follows: i. After the third matrix asphalt heated to a fluid state is mixed with the medium component and the light component, hydrogen is added for hydrogenation treatment; ii. The material obtained in step i is subjected to atmospheric and vacuum distillation to obtain a pretreated component.
14. The preparation method according to claim 13, characterized in that: In step i, the operating conditions of the hydrotreatment are: reaction temperature of 365°C to 390°C, reaction pressure of 12MPa to 22MPa, volume space velocity of 0.5 to 1.8h -1 , hydrogen-to-oil volume ratio is 400-1500; the preferred operating conditions are: reaction temperature is 370°C-390°C, reaction pressure is 13MPa-20MPa, volume space velocity is 0.5-1.2h -1 , the volume ratio of hydrogen to oil is 500-1100.
15. The preparation method according to claim 13, characterized in that: The atmospheric and vacuum distillation is carried out in an atmospheric and vacuum distillation kettle, and the final temperature of the vacuum distillation is 465-540°C, preferably 485-520°C.
16. The preparation method according to claim 10, characterized in that: In step (3), the conditions for the blending treatment are: a temperature of 170 to 185° C., a blending stirring speed of 300 to 500 r / min, and a blending stirring time of 3 to 6 hours.
Citation Information
Patent Citations
Hydraulic asphalt concrete antiseepage material with large particle size
CN105152580A
Hydraulic asphalt concrete containing broken natural sand and gravel aggregates
CN106904872A
High-performance asphalt concrete and preparation method thereof
CN114409311A
Hydraulic asphalt concrete as well as preparation method and application thereof
CN115073060A