Flame-retardant PET adhesive tape and preparation method thereof
By using a combination of acrylate polymers, flame retardants, tackifying resins and crosslinking agents in PET tape, a three-dimensional network structure is constructed, which solves the problem of flammability of existing pressure-sensitive adhesives and significantly improves the bonding performance and resistance The combustion performance achieves higher cohesive strength and heat resistance.
Patent Information
- Application Number
- CN202411405321.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing pressure-sensitive adhesives are flammable, threaten to life and property and environmental safety, and their bonding and high temperature resistance are insufficient.
Using pressure-sensitive adhesives including acrylate polymers, flame retardants, tackifying resins and crosslinking agents, a three-dimensional network structure is constructed to improve bonding by combining alkenyl siloxanes and multifunctional aziridine crosslinking agents. Performance and flame retardant capability, and improve dispersion and thermal stability by modifying flame retardant.
It significantly improves the cohesive strength, heat resistance and flame retardant properties of pressure-sensitive adhesives, achieves better bonding and flame retardant effects, and enhances the safety and application performance of PET tape.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant pressure-sensitive adhesives, in particular to a flame-retardant PET tape and a preparation method thereof. Background Art
[0002] The tape consists of two parts: a substrate and an adhesive, and connects two or more unconnected objects through bonding. In conventional applications, pressure-sensitive adhesives are usually selected as adhesives. Pressure-sensitive adhesives are a type of adhesive that can quickly adhere to the surface of a material after applying slight pressure. They are widely used in packaging, labels, electronic equipment and other fields. Among them, acrylic pressure-sensitive adhesives have good pressure sensitivity and fluidity, good wetting ability on the substrate, can quickly adhere to various substrates, and have excellent comprehensive performance. However, its main components are carbon, hydrogen, and oxygen, which are easy to burn and will cause serious damage to people’s lives, property safety and the environment. Therefore, we propose a flame-retardant PET tape and a preparation method thereof. Summary of the invention
[0003] The object of the present invention is to provide a flame retardant PET tape and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a flame retardant PET tape, comprising a PET substrate and a pressure-sensitive adhesive layer arranged on the surface of the PET substrate.
[0005] Furthermore, the pressure-sensitive adhesive layer is formed by coating the pressure-sensitive adhesive and then drying it.
[0006] Furthermore, the pressure-sensitive adhesive comprises the following components: an acrylate polymer, a flame retardant, a tackifying resin and a cross-linking agent.
[0007] Furthermore, the pressure-sensitive adhesive comprises the following components by mass: 100 parts of acrylate polymer, 20 to 30 parts of tackifying resin, 5 to 10 parts of flame retardant and 0.5 to 3.0 parts of cross-linking agent.
[0008] Further, the acrylate polymer comprises the following components by mass: 40 to 50 parts of butyl acrylate, 6 to 10 parts of methyl acrylate, 2 to 8 parts of isooctyl acrylate, 0.5 to 1.0 parts of acrylic acid, 0.5 to 1.5 parts of hydroxyethyl acrylate, 0.5 to 2.0 parts of alkenyl siloxane, 0.05 to 0.15 parts of initiator, and 40 to 60 parts of solvent;
[0009] The alkenyl siloxane is one of polydimethylmethylvinylsiloxane, allyltrimethoxysilane, 3-butylenetriethoxysilane, diethoxydivinylsilane, 5-hexenyltrimethoxysilane and 7-octenyltrimethoxysilane;
[0010] The initiator is one of benzoyl peroxide and azobisisobutyronitrile;
[0011] The solvent is one of ethyl acetate, butyl acetate and butanone.
[0012] In the above technical scheme, isooctyl acrylate and butyl acrylate are soft monomers to construct the soft segment of the acrylate polymer molecular chain, realize the bonding performance of the pressure-sensitive adhesive, and promote the wetting and spreading of the pressure-sensitive adhesive on the surface of the substrate. Methyl acrylate is a hard monomer to construct the hard segment of the acrylate polymer molecular chain, which can improve the cohesive strength of the pressure-sensitive adhesive. Acrylic acid and hydroxyethyl acrylate are functional monomers to introduce reactive groups into the molecular chain of the acrylate polymer to realize the chemical reaction with the cross-linking agent in the subsequent process, form a three-dimensional network cross-linking structure, and improve the cohesive strength of the pressure-sensitive adhesive layer. Alkenyl siloxane is introduced into the acrylate polymer molecular chain as a comonomer, which can improve its flexibility, high temperature resistance, etc., and the prepared pressure-sensitive adhesive has better bonding performance and flame retardancy.
[0013] Furthermore, the flame retardant is a mixture of one or more of ammonium polyphosphate, aluminum hydroxide, magnesium hydroxide, hydrotalcite, aluminum hypophosphite, and zinc borate.
[0014] In the above technical solution, the flame retardant is added as an additive component to the pressure-sensitive adhesive, which can generate water and flame-retardant gas at high temperature, promote carbonization, form a protective layer, prevent the spread of flames, and achieve the flame retardant effect of the pressure-sensitive adhesive. It can also improve the rheological properties of the pressure-sensitive adhesive, and improve its bonding properties and cohesive strength.
[0015] Furthermore, the tackifying resin is one of rosin resin and terpene phenol resin, or a mixture of the two.
[0016] In the above technical solution, the tackifying resin is added to improve the initial adhesion and peeling performance of the pressure-sensitive adhesive; and can participate in the cross-linking reaction of the cross-linking agent in the subsequent process to further improve the cohesive strength of the pressure-sensitive adhesive layer.
[0017] Furthermore, the cross-linking agent is a multifunctional aziridine cross-linking agent;
[0018] The crosslinking agent is a mixture of one or more of trimethylolpropane-tris[3-(2-methylaziridinyl) propionate], trimethylolpropane-tris(3-aziridinyl propionate), and pentaerythritol tris(3-aziridinyl) propionate.
[0019] In the above technical scheme, the aziridine crosslinking agent is used to react with the active groups (hydroxyl, carboxyl) in the acrylic ester polymer and the tackifying resin to construct the three-dimensional network molecular structure of the pressure-sensitive adhesive, thereby increasing its crosslinking degree, which helps to improve the strength and heat resistance of the pressure-sensitive adhesive layer.
[0020] A method for preparing a flame-retardant PET tape comprises the following processes:
[0021] Mixing acrylate monomer and alkenyl siloxane in a solvent with a mass component of 50% to 70%, stirring and heating to 70 to 80°C, adding 30% to 50% of the mass component of an initiator, and reflux reaction for 60 to 90 minutes; slowly adding the remaining initiator within 60 to 90 minutes, continuing the reaction for 100 to 150 minutes, cooling to 30 to 40°C, filtering, and adding the remaining solvent to obtain an acrylate polymer; adding a flame retardant, a tackifying resin and a crosslinking agent in sequence, stirring, and obtaining a pressure-sensitive adhesive;
[0022] The pressure-sensitive adhesive is coated on the surface of the PET substrate and dried to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0023] Furthermore, the acrylate monomers include butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, and hydroxyethyl acrylate.
[0024] Further, the coating thickness is 10 to 30 μm;
[0025] The drying conditions are: temperature 120-140°C, time 3-5 minutes.
[0026] Furthermore, the acrylic ester polymer further comprises: 8 to 16 parts of olefinic flame retardant monomers.
[0027] Further, the olefinic flame retardant monomer is prepared by the following process:
[0028] Step 1, tris (2-hydroxyethyl) isocyanurate and polyformaldehyde are mixed in anhydrous dioxane, stirred and reacted for 150 to 180 minutes at a temperature of 20 to 35° C.; DOPO is added and mixed, the temperature is raised to 50 to 70° C., and the reaction is carried out for 3 to 5 hours; the temperature is raised to 80 to 92° C., and the reaction is carried out for 2 to 4 hours; rotary evaporation, washing, and drying are performed to obtain polyhydroxy DOPO;
[0029] Step 2, polyhydroxy DOPO and trimethylamine are mixed in dichloromethane, sulfonyl chloride is slowly added over 10 minutes, and the mixture is stirred for reaction for 6 to 12 hours; washing and vacuum drying are performed to obtain a DOPO derivative;
[0030] The DOPO derivative and vinyl imidazole are mixed in dichloromethane, the temperature is raised to 80-85° C., and the mixture is stirred for reaction for 48-60 hours; the mixture is washed, precipitated, and dried to obtain an olefinic flame retardant monomer.
[0031] Furthermore, in step 1, the molar ratio of tris(2-hydroxyethyl)isocyanurate, paraformaldehyde, and DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) is 1:(3-6):(3-6);
[0032] The ratio of tris(2-hydroxyethyl)isocyanurate to dioxane is (3 to 8) g / 100 mL.
[0033] Further, in step 2, the sulfonyl chloride is one of p-methanesulfonyl chloride, pyrazole-4-sulfonyl chloride, imidazole-4-sulfonyl chloride, pyrazine-2-sulfonyl chloride, quinoline-8-sulfonyl chloride, 2-thiazolesulfonyl chloride, piperidine-1-sulfonyl chloride, isoquinoline-5-sulfonyl chloride, and quinoxaline-6-sulfonyl chloride;
[0034] The mass ratio of polyhydroxy DOPO, sulfonyl chloride and trimethylamine is 1:(0.45-0.66):(0.15-0.18);
[0035] The ratio of polyhydroxy DOPO to dichloromethane is (10-12) g / 100 mL.
[0036] Furthermore, in step 3, the mass ratio of the DOPO derivative to vinyl imidazole (1-vinylimidazole) is 10:(5.0-10.1);
[0037] The ratio of DOPO derivative to dichloromethane was 5 g / 100 mL.
[0038] In the above technical scheme, the amino group in tris(2-hydroxyethyl)isocyanurate is grafted with DOPO through polyformaldehyde, and DOPO is introduced into the triazine structure with branched hydroxyl groups to obtain polyhydroxy DOPO. The triazine and DOPO in its structure have flame retardancy, can absorb heat and decompose, promote the formation of carbon layer, cooperate with alkenylsiloxane to build a stable carbon layer, isolate the transfer of oxygen and heat; capture free radicals, interrupt the combustion chain reaction; thereby inhibiting the spread of flames, preventing further decomposition and combustion of the tape, exerting its gas phase and condensed phase flame retardant effect, and achieving the flame retardant effect of pressure-sensitive adhesive. Polyhydroxy DOPO is mixed with sulfonyl chloride, and the two are grafted through the reaction between hydroxyl and sulfonyl chloride groups to obtain DOPO derivatives. Its molecular structure has excellent stability, can absorb heat, decompose to produce non-combustible gas, reduce the temperature of the combustion system, and help improve the flame retardant grade of the tape. The introduction of sulfonates can promote the formation of phenolic compounds and aromatic compounds, absorb heat, inhibit combustion reactions, and delay combustion. The DOPO derivative is reacted with vinyl imidazole to form an ionic liquid, and a vinyl functional group is introduced, which is recorded as an olefinic flame retardant monomer. The olefinic flame retardant monomer has a trifunctional vinyl group and is introduced into the polymerization monomer of the acrylate polymer, which helps to construct a polymer network. The ionic liquid properties of the olefinic flame retardant monomer enable it to form an ionic network, which helps to improve the thermal stability of the pressure-sensitive adhesive, thereby improving the strength, heat resistance and flame retardancy of the pressure-sensitive adhesive layer.
[0039] Furthermore, the flame retardant is modified, and the modification process is as follows:
[0040] The olefin flame retardant monomer and dopamine hydrochloride are mixed in a buffer solution and stirred for 1 to 6 hours to obtain a modifier; the modifier is sprayed on the surface of the flame retardant, allowed to stand, and dried to obtain a modified flame retardant.
[0041] Furthermore, the mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is (1-3):10;
[0042] The ratio of dopamine hydrochloride to buffer solution is (0.2-0.3) g / 100 mL;
[0043] The buffer solution was 10 mM Tris buffer, pH 8.5.
[0044] Furthermore, the mass ratio of the flame retardant to the modifier is 10:(1-3).
[0045] In the above technical scheme, the oxidative self-polymerization of dopamine is free radical polymerization, and its self-polymerization in the buffer generates free radicals, which can initiate the polymerization reaction of the olefinic flame retardant monomer, so that it is deposited together with dopamine on the surface of the flame retardant, thereby preparing a modified flame retardant, which helps to improve the dispersibility of the flame retardant in the acrylate polymer, reduce its solubility and water absorption, and improve its thermal stability and flame retardancy.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] 1. The present invention describes a flame-retardant PET tape and a preparation method thereof. A flame-retardant ionic liquid olefinic flame-retardant monomer is prepared by using tris (2-hydroxyethyl) isocyanurate, polyformaldehyde, DOPO, sulfonyl chloride, and vinyl imidazole as raw materials, and the olefinic flame-retardant monomer is introduced into an acrylic ester polymer, so that the pressure-sensitive adhesive has better strength and flame retardancy.
[0048] 2. The flame-retardant PET tape and preparation method thereof described in the present invention initiates polymerization of olefinic flame-retardant monomers through self-polymerization of dopamine, so that the flame retardants are co-deposited on the surface of the flame retardant to obtain a modified flame retardant, thereby improving the dispersibility of the flame retardant in the acrylate polymer and reducing its water absorption, which helps to further improve the thermal stability and flame retardant ability of the flame retardant. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] In the following specific implementations,
[0051] The thickness of the PET substrate is 25 μm;
[0052] The flame retardant is a mixture of ammonium polyphosphate and aluminum hydroxide (nano-grade), with a mass ratio of 3:2;
[0053] Ammonium polyphosphate, nano-aluminum hydroxide: from Xiens Biochemical Technology Co., Ltd.;
[0054] The tackifying resin is a mixture of rosin resin and terpene phenol resin, with a mass ratio of 1:1;
[0055] Rosin resin: SYLVALITE RE100F; terpene phenol resin: SYLVARES TP2019, from Kraton, USA.
[0056] Embodiment 1: A method for preparing a flame-retardant PET tape, comprising the following process:
[0057] Step 1, tris(2-hydroxyethyl)isocyanurate and polyformaldehyde are mixed in anhydrous dioxane, stirred and reacted for 180 minutes at a temperature of 20°C; DOPO is added and mixed, the temperature is raised to 50°C, and the reaction is carried out for 5 hours; the temperature is raised to 80°C, and the reaction is carried out for 4 hours; rotary evaporation, washing, and drying are performed to obtain polyhydroxy DOPO; the molar ratio of tris(2-hydroxyethyl)isocyanurate, polyformaldehyde, and DOPO is 1:3:3; the ratio of tris(2-hydroxyethyl)isocyanurate and dioxane is 8g / 100mL;
[0058] Mix polyhydroxy DOPO and trimethylamine in dichloromethane, slowly add sulfonyl chloride, add it over 10 minutes, stir and react for 6 hours; wash and vacuum dry to obtain a DOPO derivative; the sulfonyl chloride is p-methylsulfonyl chloride; the mass ratio of polyhydroxy DOPO, sulfonyl chloride and trimethylamine is 1:0.50:0.16; the ratio of polyhydroxy DOPO and dichloromethane is 12g / 100mL;
[0059] Mix DOPO derivative and 1-vinylimidazole in dichloromethane, heat to 80°C, and stir to react for 48 hours; wash, precipitate, and dry to obtain an olefinic flame retardant monomer; the mass ratio of DOPO derivative and 1-vinylimidazole is 10:5; the ratio of DOPO derivative and dichloromethane is 5g / 100mL;
[0060] Step 2, mixing the olefinic flame retardant monomer and dopamine hydrochloride in a buffer solution (10mM Tris buffer, pH 8.5), stirring for 1h to obtain a modifier; spraying on the surface of the flame retardant, standing, and drying to obtain a modified flame retardant; the mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is 1:10; the ratio of dopamine hydrochloride and buffer solution is 0.2g / 100mL; the mass ratio of the flame retardant and the modifier is 10:1;
[0061] Step 3, butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, alkenyl siloxane, alkenyl flame retardant monomer, mixed in a 50% component weight solvent, stirred and heated to 80°C, added 30% component weight initiator, refluxed for 60 minutes; slowly added the remaining initiator, added within 60 minutes, continued to react for 100 minutes, cooled to 30°C, filtered, added the remaining solvent, and obtained an acrylate polymer; added a modified flame retardant, a tackifying resin and a crosslinking agent in sequence, stirred, and obtained a pressure-sensitive adhesive; the pressure-sensitive adhesive includes the following qualities: Components: 100 parts of acrylate polymer, 20 parts of tackifying resin, 5 parts of modified flame retardant and 0.5 parts of crosslinking agent; the acrylate polymer includes the following mass components: 40 parts of butyl acrylate, 6 parts of methyl acrylate, 2 parts of isooctyl acrylate, 0.5 parts of acrylic acid, 0.5 parts of hydroxyethyl acrylate, 0.5 parts of alkenyl siloxane, 0.05 parts of initiator azobisisobutyronitrile, 60 parts of solvent ethyl acetate and 8 parts of alkenyl flame retardant monomer; the alkenyl siloxane is allyltrimethoxysilane; the crosslinking agent is trimethylolpropane-tris[3-(2-methylaziridinyl) propionate];
[0062] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 120° C. for 4 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0063] Embodiment 2: A method for preparing a flame-retardant PET tape, comprising the following process:
[0064] Step 1, tris(2-hydroxyethyl)isocyanurate and polyformaldehyde are mixed in anhydrous dioxane, stirred and reacted for 165 minutes at 27°C; DOPO is added and mixed, the temperature is raised to 60°C, and the reaction is carried out for 4 hours; the temperature is raised to 86°C, and the reaction is carried out for 3 hours; rotary evaporation, washing, and drying are performed to obtain polyhydroxy DOPO; the molar ratio of tris(2-hydroxyethyl)isocyanurate, polyformaldehyde, and DOPO is 1:5:5; the ratio of tris(2-hydroxyethyl)isocyanurate and dioxane is 5g / 100mL;
[0065] Mix polyhydroxy DOPO and trimethylamine in dichloromethane, slowly add sulfonyl chloride, add it over 10 minutes, stir and react for 9 hours; wash and vacuum dry to obtain a DOPO derivative; the sulfonyl chloride is imidazole-4-sulfonyl chloride; the mass ratio of polyhydroxy DOPO, sulfonyl chloride and trimethylamine is 1:0.47:0.17; the ratio of polyhydroxy DOPO and dichloromethane is 11g / 100mL;
[0066] Mix DOPO derivative and 1-vinylimidazole in dichloromethane, heat to 82°C, and stir to react for 54 hours; wash, precipitate, and dry to obtain an olefinic flame retardant monomer; the mass ratio of DOPO derivative and 1-vinylimidazole is 10:7.5; the ratio of DOPO derivative and dichloromethane is 5g / 100mL;
[0067] Step 2, mixing the olefinic flame retardant monomer and dopamine hydrochloride in a buffer solution (10mM Tris buffer, pH 8.5), stirring for 4h to obtain a modifier; spraying on the surface of the flame retardant, standing, and drying to obtain a modified flame retardant; the mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is 2:10; the ratio of dopamine hydrochloride and buffer solution is 0.25g / 100mL; the mass ratio of the flame retardant and the modifier is 10:2;
[0068] Step 3, butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, alkenyl siloxane, alkenyl flame retardant monomer, mixed in a solvent with a mass percentage of 60%, stirred and heated to 80°C, added an initiator with a mass percentage of 40%, refluxed for 75 minutes; slowly added the remaining initiator within 75 minutes, continued the reaction for 120 minutes, cooled to 35°C, filtered, added the remaining solvent, and obtained an acrylate polymer; added a modified flame retardant, a tackifying resin, and a crosslinking agent in sequence, stirred, and obtained a pressure-sensitive adhesive; the pressure-sensitive adhesive comprises the following Components by mass: 100 parts of acrylate polymer, 20 parts of tackifying resin, 8 parts of modified flame retardant and 1.8 parts of crosslinking agent; acrylate polymer includes the following components by mass: 45 parts of butyl acrylate, 8 parts of methyl acrylate, 5 parts of isooctyl acrylate, 0.8 parts of acrylic acid, 1 part of hydroxyethyl acrylate, 1.2 parts of alkenyl siloxane, 0.10 parts of initiator azobisisobutyronitrile, 50 parts of solvent ethyl acetate and 12 parts of alkenyl flame retardant monomer; alkenyl siloxane is 5-hexenyltrimethoxysilane; crosslinking agent is trimethylolpropane-tris(3-aziridinyl propionate);
[0069] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 130° C. for 4 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0070] Embodiment 3: A method for preparing a flame-retardant PET tape, comprising the following process:
[0071] Step 1, tris(2-hydroxyethyl)isocyanurate and polyformaldehyde are mixed in anhydrous dioxane, stirred and reacted for 150 minutes at a temperature of 35°C; DOPO is added and mixed, the temperature is raised to 70°C, and the reaction is carried out for 3 hours; the temperature is raised to 92°C, and the reaction is carried out for 2 hours; rotary evaporation, washing, and drying are performed to obtain polyhydroxy DOPO; the molar ratio of tris(2-hydroxyethyl)isocyanurate, polyformaldehyde, and DOPO is 1:6:6; the ratio of tris(2-hydroxyethyl)isocyanurate and dioxane is 3g / 100mL;
[0072] Mix polyhydroxy DOPO and trimethylamine in dichloromethane, slowly add sulfonyl chloride, add it over 10 minutes, stir and react for 12 hours; wash and vacuum dry to obtain a DOPO derivative; the sulfonyl chloride is quinoxaline-6-sulfonyl chloride; the mass ratio of polyhydroxy DOPO, sulfonyl chloride and trimethylamine is 1:0.66:0.17; the ratio of polyhydroxy DOPO and dichloromethane is 12g / 100mL
[0073] Mix DOPO derivative and 1-vinylimidazole in dichloromethane, heat to 85°C, and stir to react for 60 hours; wash, precipitate, and dry to obtain an olefinic flame retardant monomer; the mass ratio of DOPO derivative and 1-vinylimidazole is 10:10.1; the ratio of DOPO derivative and dichloromethane is 5g / 100mL;
[0074] Step 2, mixing the olefinic flame retardant monomer and dopamine hydrochloride in a buffer solution (10mM Tris buffer, pH 8.5), stirring for 6h to obtain a modifier; spraying on the surface of the flame retardant, standing, and drying to obtain a modified flame retardant; the mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is 3:10; the ratio of dopamine hydrochloride and buffer solution is 0.3g / 100mL; the mass ratio of the flame retardant and the modifier is 10:3;
[0075] Step 3, butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, alkenyl siloxane, alkenyl flame retardant monomer, mixed in a solvent with a mass percentage of 70%, stirred and heated to 80°C, added an initiator with a mass percentage of 50%, and refluxed for 90 minutes; slowly added the remaining initiator within 90 minutes, continued the reaction for 150 minutes, cooled to 40°C, filtered, and added the remaining solvent to obtain an acrylate polymer; added a modified flame retardant, a tackifying resin, and a crosslinking agent in sequence, stirred, and obtained a pressure-sensitive adhesive; the pressure-sensitive adhesive includes the following materials: The components by mass are: 100 parts of acrylate polymer, 20 parts of tackifying resin, 10 parts of modified flame retardant and 3.0 parts of crosslinking agent; the acrylate polymer includes the following mass components: 50 parts of butyl acrylate, 10 parts of methyl acrylate, 8 parts of isooctyl acrylate, 1.0 parts of acrylic acid, 1.5 parts of hydroxyethyl acrylate, 2.0 parts of alkenyl siloxane, 0.15 parts of initiator azobisisobutyronitrile, 40 parts of solvent ethyl acetate and 16 parts of alkenyl flame retardant monomer; the alkenyl siloxane is polydimethyl methylvinyl siloxane; the crosslinking agent is pentaerythritol tris (3-aziridinyl) propionate;
[0076] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 140° C. for 5 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0077] Comparative Example 1: A method for preparing a flame-retardant PET tape, comprising the following process:
[0078] Step 1, tris(2-hydroxyethyl)isocyanurate and trimethylamine are mixed in dichloromethane, sulfonyl chloride is slowly added, the addition is completed within 10 minutes, and the reaction is stirred for 6 hours; washing, vacuum drying, and obtaining a DOPO derivative; the sulfonyl chloride is p-methylsulfonyl chloride; the mass ratio of tris(2-hydroxyethyl)isocyanurate, sulfonyl chloride, and trimethylamine is 1:2.24:0.68; the ratio of tris(2-hydroxyethyl)isocyanurate to dichloromethane is 12 g / 100 mL;
[0079] The triazine derivative and 1-vinylimidazole were mixed, heated to 80°C, and stirred for reaction for 48 hours; washed, precipitated, and dried to obtain an olefinic flame retardant monomer; the mass ratio of the triazine derivative and 1-vinylimidazole was 10:5.0; the ratio of the triazine derivative and dichloromethane was 5g / 100mL;
[0080] Step 2, mixing the olefinic flame retardant monomer and dopamine hydrochloride in a buffer solution (10mM Tris buffer, pH 8.5), stirring for 1h to obtain a modifier; spraying on the surface of the flame retardant, standing, and drying to obtain a modified flame retardant; the mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is 1:10; the ratio of dopamine hydrochloride and buffer solution is 0.2g / 100mL; the mass ratio of the flame retardant and the modifier is 10:1;
[0081] Step 3 is the same as in Example 1, obtaining a pressure-sensitive adhesive;
[0082] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 120° C. for 4 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0083] Comparative Example 2: A method for preparing a flame-retardant PET tape, comprising the following process:
[0084] Step 1, trimethylolpropane triacrylate and dopamine hydrochloride are mixed in a buffer solution (10mM Tris buffer, pH 8.5), stirred for 1h to obtain a modifier; sprayed on the surface of the flame retardant, allowed to stand, and dried to obtain a modified flame retardant; the mass ratio of the olefinic flame retardant monomer to dopamine hydrochloride is 1:10; the ratio of dopamine hydrochloride to the buffer solution is 0.2g / 100mL; the mass ratio of the flame retardant to the modifier is 10:1;
[0085] Step 2, butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, alkenyl siloxane, trimethylolpropane triacrylate, mixed in a 50% component weight solvent, stirred and heated to 80°C, added 30% component weight initiator, refluxed for 60 minutes; slowly added the remaining initiator, added within 60 minutes, continued to react for 100 minutes, cooled to 30°C, filtered, added the remaining solvent, and obtained an acrylate polymer; added a modified flame retardant, a tackifying resin and a crosslinking agent in sequence, stirred, A pressure-sensitive adhesive is obtained; the pressure-sensitive adhesive comprises the following components by mass: 100 parts of acrylate polymer, 20 parts of tackifying resin, 5 parts of modified flame retardant and 0.5 parts of cross-linking agent; the acrylate polymer comprises the following components by mass: 40 parts of butyl acrylate, 6 parts of methyl acrylate, 2 parts of isooctyl acrylate, 0.5 parts of acrylic acid, 0.5 parts of hydroxyethyl acrylate, 0.5 parts of alkenyl siloxane, 0.05 parts of initiator azobisisobutyronitrile, 60 parts of solvent ethyl acetate and 8 parts of trimethylolpropane triacrylate; the alkenyl siloxane is allyltrimethoxysilane;
[0086] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 120° C. for 4 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0087] Comparative Example 3: A method for preparing a flame-retardant PET tape, comprising the following process:
[0088] Butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, hydroxyethyl acrylate, alkenyl siloxane are mixed in a solvent with a mass percentage of 50%, stirred and heated to 80°C, an initiator with a mass percentage of 30% is added, and the reaction is refluxed for 60 minutes; the remaining initiator is slowly added within 60 minutes, the reaction is continued for 100 minutes, the mixture is cooled to 30°C, filtered, and the remaining solvent is added to obtain an acrylate polymer; a modified flame retardant, a tackifying resin and a crosslinking agent are added in sequence, stirred to obtain a pressure-sensitive adhesive; the pressure-sensitive adhesive comprises the following mass components: 100 parts of acrylate polymer, 20 parts of tackifying resin, 5 parts of flame retardant and 0.5 parts of crosslinking agent; the acrylate polymer comprises the following mass components: 40 parts of butyl acrylate, 6 parts of methyl acrylate, 2 parts of isooctyl acrylate, 0.5 parts of acrylic acid, 0.5 parts of hydroxyethyl acrylate, 0.5 parts of alkenyl siloxane, 0.05 parts of initiator azobisisobutyronitrile, and 60 parts of solvent ethyl acetate; the alkenyl siloxane is allyltrimethoxysilane;
[0089] The pressure-sensitive adhesive was coated on the surface of the PET substrate with a coating thickness of 25 μm, and dried at a temperature of 120° C. for 4 minutes to form a pressure-sensitive adhesive layer to obtain a PET tape.
[0090] Experiment: Take the flame-retardant PET tapes obtained in Examples 1-3 and Comparative Examples 1-3, prepare samples, test their properties respectively and record the test results:
[0091] Adhesion test: GB / T 4851 is used as the reference standard to test the adhesion of the sample. The test temperature is 23°C, the relative humidity is 65%, and the weight is 1kg.
[0092] Flame retardant performance test: Using ASTMD 2863 as the reference standard, the limiting oxygen index (LOI) of the pressure-sensitive adhesive layer sample was tested, and the sample size was 80mm×10mm×4mm.
[0093] Holding force(h) LOI(%) Example 1 49.6 30.6 Example 2 50.8 31.8 Example 3 51.2 32.5 Comparative Example 1 46.1 28.3 Comparative Example 2 32.7 25.9 Comparative Example 3 27.8 25.2
[0094] According to the data in the above table, we can clearly draw the following conclusions:
[0095] The PET tapes obtained in Examples 1-3 are compared with the PET tapes obtained in Comparative Examples 1-3. The test results show that:
[0096] Compared with the comparative example, the flame-retardant PET tapes obtained in Examples 1-3 have higher holding force data and limiting oxygen index data of the pressure-sensitive adhesive layer, which fully demonstrates that the present invention achieves the improvement of the cohesive strength and flame retardant performance of the pressure-sensitive adhesive layer and achieves the flame retardant performance of the prepared PET tape.
[0097] Compared with Example 1, the alkenyl flame retardant monomer in Comparative Example 1 is prepared from tris(2-hydroxyethyl)isocyanurate, sulfonyl chloride and 1-vinylimidazole. In Comparative Example 2, the alkenyl flame retardant monomer is replaced with trimethylolpropane triacrylate. In Comparative Example 3, the alkenyl flame retardant monomer component is not set. The PET tapes obtained in Examples 1-3 have decreased adhesion data and limiting oxygen index data of the pressure-sensitive adhesive layer. It can be seen that the setting of the pressure-sensitive adhesive component and its process of the present invention can promote the improvement of its cohesive strength and flame retardant properties.
[0098] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A method for preparing a flame retardant PET tape, characterized in that: Including the following processes: The acrylate monomer, alkenyl siloxane and alkenyl flame retardant monomer are mixed in a solvent with a mass component of 50% to 70%, stirred and heated to 70 to 80°C, and an initiator with a mass component of 30% to 50% is added, and the reaction is refluxed for 60 to 90 minutes; the remaining initiator is slowly added within 60 to 90 minutes, and the reaction is continued for 100 to 150 minutes, and the mixture is cooled to 30 to 40°C, filtered, and the remaining solvent is added to obtain an acrylate polymer; a flame retardant, a tackifying resin and a cross-linking agent are added in sequence, stirred to obtain a pressure-sensitive adhesive; the pressure-sensitive adhesive is coated on the surface of a PET substrate, dried to form a pressure-sensitive adhesive layer, and a PET tape is obtained; The olefinic flame retardant monomer is prepared by the following process: Step 1, tris (2-hydroxyethyl) isocyanurate and polyformaldehyde are mixed in anhydrous dioxane, stirred and reacted for 150 to 180 minutes at a temperature of 20 to 35° C.; DOPO is added and mixed, the temperature is raised to 50 to 70° C., and the reaction is carried out for 3 to 5 hours; the temperature is raised to 80 to 92° C., and the reaction is carried out for 2 to 4 hours to obtain polyhydroxy DOPO; Step 2, polyhydroxy DOPO and trimethylamine are mixed in dichloromethane, and sulfonyl chloride is slowly added over 10 minutes, and the mixture is stirred for reaction for 6 to 12 hours to obtain a DOPO derivative; The DOPO derivative and 1-vinylimidazole are mixed in dichloromethane, the temperature is raised to 80-85° C., and the mixture is stirred for reaction for 48-60 hours to obtain an olefinic flame retardant monomer.
2. The method for preparing a flame retardant PET tape according to claim 1, characterized in that: In the step 1, the molar ratio of tris(2-hydroxyethyl)isocyanurate, paraformaldehyde and DOPO is 1:(3-6):(3-6).
3. The method for preparing a flame retardant PET tape according to claim 1, characterized in that: In the step 2, the sulfonyl chloride is one of p-methanesulfonyl chloride, pyrazole-4-sulfonyl chloride, imidazole-4-sulfonyl chloride, pyrazine-2-sulfonyl chloride, quinoline-8-sulfonyl chloride, 2-thiazolesulfonyl chloride, piperidine-1-sulfonyl chloride, isoquinoline-5-sulfonyl chloride, and quinoxaline-6-sulfonyl chloride; The mass ratio of polyhydroxy DOPO, sulfonyl chloride and trimethylamine is 1:(0.45-0.66):(0.15-0.18).
4. The method for preparing a flame-retardant PET tape according to claim 1, characterized in that: In the step 2, the mass ratio of the DOPO derivative to 1-vinylimidazole is 10:(5.0-10.1).
5. The method for preparing a flame retardant PET tape according to claim 1, characterized in that: The flame retardant is a mixture of one or more of ammonium polyphosphate, aluminum hydroxide, magnesium hydroxide, hydrotalcite, aluminum hypophosphite, and zinc borate.
6. The method for preparing a flame retardant PET tape according to claim 1, characterized in that: The flame retardant is modified, and the modification process is as follows: The olefin flame retardant monomer and dopamine hydrochloride are mixed in a buffer solution and stirred for 1 to 6 hours to obtain a modifier; the modifier is sprayed on the surface of the flame retardant, allowed to stand, and dried to obtain a modified flame retardant.
7. The method for preparing a flame-retardant PET tape according to claim 6, characterized in that: The mass ratio of the olefinic flame retardant monomer and dopamine hydrochloride is (1-3):10; The mass ratio of flame retardant to modifier is 10:(1-3).
8. The method for preparing a flame-retardant PET tape according to claim 1, characterized in that: The pressure-sensitive adhesive comprises the following components by mass: 100 parts of acrylate polymer, 20 to 30 parts of tackifying resin, 5 to 10 parts of flame retardant and 0.5 to 3.0 parts of cross-linking agent.
9. The method for preparing a flame-retardant PET tape according to claim 8, characterized in that: The acrylate monomers include butyl acrylate, methyl acrylate, isooctyl acrylate, acrylic acid, and hydroxyethyl acrylate; the acrylate polymer includes the following components by mass: 40 to 50 parts of butyl acrylate, 6 to 10 parts of methyl acrylate, 2 to 8 parts of isooctyl acrylate, 0.5 to 1.0 part of acrylic acid, 0.5 to 1.5 parts of hydroxyethyl acrylate, 0.5 to 2.0 parts of alkenyl siloxane, 8 to 16 parts of alkenyl flame retardant monomers, 0.05 to 0.15 parts of initiators, and 40 to 60 parts of solvents.
10. A flame retardant PET tape prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
DOPO flame retardant compositions
CN101663374A
Phenolic resin containing tri(2-hydroxyethyl)isocyanurate and preparation method of phenolic resin
CN106751440A
Modified mullite, water-based intumescent fire retardant coating and preparation methods of modified mullite and water-based intumescent fire retardant coating
CN113667188A
PET pressure-sensitive adhesive tape
CN114517063A
Phosphorus-containing halogen-free flame-retardant polyacrylate pressure-sensitive adhesive and preparation method thereof
CN117070167A
Cited By
TPU wire rod and preparation method thereof
CN119490739A
Flame-retardant adhesive tape for lithium battery edge covering and preparation method of flame-retardant adhesive tape