Method for preventing casting residues from being bonded in heavy ladle through cluster jet flow oxygen lance
Through the flame impact and combustion of the cast residual residue and sticky slag by the cluster jet oxygen gun, the problem of sticking caused by the temperature drop of the cast residual residue is solved, ensuring the high temperature state of the cast residual residue and the continuity of the return production process, and improving the The economic and environmental benefits of steel mills.
Patent Information
- Application Number
- CN202310661284.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
During the steel production process, the cast residue is easily stuck due to temperature drop after pouring into the molten iron bag, which affects the subsequent operation of the molten iron bag and the continuity of the cast residue return production process, increasing production costs and operating losses.
The cluster jet oxygen gun is used to flame impact the cast residue and sticky slag on the surface of the heavy-pack molten iron bag, heat and melt it, and exothermic the combustion of CO and O2 to promote the full contact and stirring of the cast residue and molten iron to avoid sticking. Assist and solidify.
It effectively avoids the phenomenon of cast residue sticking on the inner wall of the molten iron bag, ensures the temperature of cast residue keeps it, promotes its return to production and utilization, and improves production efficiency and economic benefits.
Smart Images

Figure CN119082385A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling steel slag, and in particular to a method for preventing casting slag from sticking to a heavy-clad iron ladle by using a clustered jet oxygen lance. Background Art
[0002] In the long process of steel production, in the blast furnace-converter process, after the molten steel on the continuous casting platform is cast, there will always be a part of the molten steel and hot slag left in the ladle on the platform that cannot be put into the middle ladle. This is to ensure the quality of the subsequent continuous casting billets. The remaining hot melt in the ladle is usually the casting slag in a broad sense.
[0003] The broad sense of the casting slag contains two parts of melt, one is the liquid metal part in the broad sense of the casting slag - that is, molten steel, and the other is the liquid slag part in the broad sense of the casting slag - that is, the narrow sense of the casting slag. Since the density of the molten steel in the broad sense of the casting slag and the narrow sense of the casting slag is quite different, the density of the molten steel is much greater than that of the narrow sense of the casting slag, so usually the bottom of the ladle is molten steel, and the narrow sense of the casting slag is above the molten steel.
[0004] For a 300t converter steel plant, there are usually 6-10t of broad casting slag, of which molten steel and narrow casting slag each account for half, that is, there are 3-5t of molten steel and 3-5t of narrow casting slag in the casting ladle. Because this part of the melt contains valuable refined molten steel and has huge thermal energy, returning the broad casting slag to production can achieve higher productivity, higher production benefits and significant energy-saving and consumption-reducing advantages.
[0005] In the existing generalized casting slag recycling technology, there are several return paths: one is to return to the refining furnace, the second is to return to the converter, and the third is to return to the desulfurization process. Among them, the second and third paths both require pouring the generalized casting slag into the ladle, and then returning the ladle to the process before the converter. This is the generalized casting slag recycling technology.
[0006] Since the return of generalized casting slag is intermittent, the interval period is usually about half an hour. Considering the temperature drop of generalized casting slag, a part of molten iron can be pre-loaded in the ladle first, and then the generalized casting slag can be collected. This ladle with pre-loaded molten iron is called a heavy-bag ladle.
[0007] For 300t converter steel plants, 30t of molten iron is usually pre-loaded in the ladle. With the heat reserve of 30t of molten iron, the ladle can receive generalized casting slag 3 to 5 times. In the interval between each time the ladle receives casting slag, the casting slag in the ladle is open to cool down. In addition, when the generalized casting slag is injected into the ladle, since the narrow casting slag in the generalized casting slag is oxidizing, it will react with the molten iron with reducing elements in the ladle, and the reaction is endothermic. In addition, the heat dissipation during the waiting period for receiving the casting slag causes the temperature of the melt in the ladle to drop, which can easily reduce the temperature of the slag in the ladle to the extent that it adheres to or condenses on the inner wall of the ladle, causing the casting slag in the ladle to stick to the ladle, which has a bad impact on the subsequent ladle pouring and pouring of the melt. The repair of the ladle after slag sticking affects the life of the ladle refractory materials, increases the production and repair costs, and more seriously affects the continuous operation of the casting slag return production process, causing multiple operating losses to the steel mill.
[0008] Therefore, how to prevent the casting slag from sticking to the ladle due to the drop in slag temperature after being poured into the ladle becomes a technical problem that needs to be solved urgently. Summary of the invention
[0009] The purpose of the present invention is to provide a method for preventing casting slag from sticking to the heavy-clad iron ladle by using a clustered jet oxygen lance, solve the problem of the casting slag sticking to the iron ladle wall and solidifying in the production process, promote the improvement of the casting slag production process, and have significant economic and environmental benefits.
[0010] To achieve the above object, the technical solution of the present invention is:
[0011] A method for preventing casting slag from sticking to a heavy-clad iron ladle by using a clustered jet oxygen lance comprises the following steps:
[0012] 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled is 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle;
[0013] 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle. When the heavy ladle iron ladle is moved, the surface casting slag in the heavy ladle iron ladle does not shake, or sticky slag is generated at the contact between the inner wall of the heavy ladle iron ladle and the surface casting slag, the surface casting slag and sticky slag are impacted with a concentrated jet oxygen gun flame, the sticky slag is heated and melted, and the casting slag in the heavy ladle iron ladle is continuously stirred and churned;
[0014] Alternatively, after the casting slag in the ladle is injected into the heavy ladle iron ladle, a cluster jet oxygen lance is immediately used to impact the surface of the casting slag;
[0015] At the same time, the CO gas and O2 that escape from the casting slag are ignited by the flame of the cluster jet oxygen lance for combustion;
[0016] Repeat the above operation until the heavy ladle completes receiving the casting slag;
[0017] 3) Casting slag transfer
[0018] The heavy iron ladle that receives the casting slag is returned to production for utilization.
[0019] Preferably, in step 2), a concentrated jet oxygen lance is used to continuously or intermittently impact the casting slag and sticky slag on the surface.
[0020] Preferably, in step 2), during the impact process, the distance between the concentrated jet oxygen lance and the casting slag does not exceed 1.2 m.
[0021] In the method of the present invention:
[0022] After the heavy-clad iron ladle takes on the casting slag, when the heavy-clad iron ladle is moved, the surface casting slag inside the heavy-clad iron ladle does not shake, or sticky slag is generated at the contact between the inner wall of the heavy-clad iron ladle and the surface casting slag, the flame of the clustered jet oxygen lance is used to impact the surface casting slag and sticky slag. The clustered jet oxygen lance is a high-speed composite jet oxygen lance that uses central oxygen supply and wraps a layer of fuel gas flow outside the central oxygen jet. It has strong firepower and can quickly heat and melt the target object, heat and melt the generated sticky slag, so that the casting slag no longer adheres to the inner wall of the iron ladle, avoiding serious slagging and sticking of the casting slag on the inner wall of the iron ladle.
[0023] Furthermore, a clustered jet oxygen lance is used to impact the surface of the casting slag. The clustered jet oxygen lance has good jet concentration, and can keep the high-speed core section of the jet concentrated without diverging over a long distance, and can maintain its strong impact force over a long distance. Therefore, the lance head does not need to be immersed in the casting slag layer to effectively impact the melt to form an impact stirring effect. Under the action of the strong impact force, the casting slag will be driven to stir and tumble, so that the casting slag and molten iron are fully in contact. The oxygen injected by the clustered jet oxygen lance reacts with [Si], [Mn], and [C] in the molten iron to release heat, thereby supplementing the heat of the casting slag and the molten iron, thereby compensating for the heat absorbed by the reaction of the highly oxidizing (FeO) in the casting slag with the reducing elements [C], [Si], and [Mn] rich in the molten iron.
[0024] At the same time, the CO gas generated by the reaction of oxygen and molten iron overflows from the melt, which will drive the melt to churn, so that the solidified slag and low-temperature slag to be effectively heated and melted, and regain good fluidity.
[0025] The CO and O2 overflowing from the melt are ignited by the clustered jet oxygen lance to form a combustion flame, which further releases heat to bake the inner wall of the ladle and the surface of the casting slag, so that the temperature of the ladle wall and the casting slag is maintained at a high temperature, reducing or eliminating the possibility of adhesion of the casting slag to the ladle wall.
[0026] The present invention utilizes the dual effects of direct melting of condensed slag by a concentrated jet oxygen lance and combustion of CO and O2 to ensure that excessive temperature drop will not occur during the production process of the casting slag, and to avoid the phenomenon of the casting slag sticking to the inner wall of the iron ladle and solidifying.
[0027] The differences and improvements of the present invention over the prior art are as follows:
[0028] Chinese patent CN2018102072178 discloses "a method for recovering molten steel by returning hot casting slag to a ladle", which receives and circulates multiple ladles of casting slag by means of a holding furnace set in the molten steel receiving span. The function of the holding furnace is to heat the casting slag by induction heating or oxygen blowing, and at least three ladles of casting slag are poured into the ladles. Since the casting slag is a poor conductor of heat, the thick slag layer cannot be heated by either induction heating or oxygen blowing. The slag layer on the upper surface will also cool down and solidify, and will not play the role of heating or heat preservation of the slag. The present invention uses a clustered jet oxygen lance to directly melt the condensed slag, combines the reaction and combustion heat release, and at the same time, stirs and churns the melt to promote heat transfer, so that the casting slag can be kept in a relatively high temperature range to avoid sticky slag solidification.
[0029] Chinese patent CN2018115574613 discloses "a method for recycling hot casting slag from ladle in converter", step 1): after the converter taps steel, the converter slag is splashed in the converter, and the converter slag is splashed and all of it remains in the converter, located at the bottom and lining of the converter; step 2): the hot metal is desulfurized and pretreated in the molten iron tank, and the hot casting slag is mixed with the molten iron after slagging and added to the converter for converter smelting. After the molten iron is pretreated and slag is removed, the temperature of the molten iron will be greatly reduced, and then the casting slag is directly poured into it. The further reaction of the casting slag and the molten iron will absorb heat, so the casting slag is easy to stick to the ladle. When pouring molten iron to the converter, the slag on the wall of the molten iron ladle will make it difficult to predict the path, direction and speed of the molten iron being poured into the converter. It is very likely that the molten iron and slag will splash everywhere, or even splash out of the converter, which will bring great danger to the operation of adding molten iron to the converter.
[0030] Chinese patent CN2010102764524 discloses "a method for recycling and reusing hot slag from continuous casting ladle". In continuous casting production, after the ladle molten steel is injected into the tundish, the molten hot slag in the ladle is poured into the heavy iron tank; then the hot slag is added to the converter together with the molten iron for steelmaking. The patent mentions that the slag may coagulate, but no solution is proposed. The present invention focuses on how to prevent the casting slag from coagulating due to continuous cooling.
[0031] Chinese patent CN2014102591190 discloses "an operation method for recovering excess slag from continuous casting in a molten iron ladle". In this patent, a heavy ladle is used to receive the excess slag. However, the amount of molten iron in the ladle must reach 70-80% of the total amount of molten iron in the ladle at the beginning, while the amount of pre-loaded molten iron in the present invention is only about 10%. Therefore, the present invention can receive excess slag from multiple ladles of casting and return it to production for utilization. The impact stirring effect of the concentrated jet oxygen lance on the melt can promote the blending and mixing of the melt and facilitate heat transfer.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention uses a clustered jet oxygen gun to impact the casting slag and sticky slag on the inner surface of the heavy-clad iron ladle, heats and melts the condensed slag, and combines the combustion heat release of CO and O2 overflowing from the melt on the slag surface, as well as the heat released by the reaction between oxygen and molten iron, to perform multiple heating on the casting slag in the heavy-clad iron ladle. The heat absorbed and lost by the reaction between molten iron and the casting slag is compensated, thereby ensuring that the temperature of the casting slag will not drop significantly. Even if one iron ladle is used to receive multiple packages of casting slag, the phenomenon of sticky slag solidification on the inner wall of the iron ladle can be avoided, which helps to continuously improve the casting slag return production technology, form a good process technology guarantee, and jointly achieve the improvement of the efficiency of the steel plant.
[0034] At the same time, the impact effect of the concentrated jet oxygen lance and the impact and stirring effect of CO and O2 overflowing from the surface of the casting slag on the melt are utilized to promote the uniform transfer of heat among the casting slags, thus avoiding the slag solidification caused by the local casting slag temperature being too low.
[0035] In order to prevent the casting slag from sticking, slagging and sticking in the production process, the prior art mainly focuses on how to quickly return the casting slag to production or improve the equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic diagram of a device according to Embodiment 1 of the present invention. DETAILED DESCRIPTION
[0037] Example 1
[0038] See also Figure 1 The method of using a clustered jet oxygen lance to prevent casting slag from sticking to a heavy iron ladle comprises the following steps:
[0039] 1) After the molten iron is filled into the ladle for standby use, the amount of molten iron filled is 10% of the molten iron volume, and the ladle filled with molten iron is called a heavy ladle 1;
[0040] 2) After the molten steel is poured, the casting slag in the ladle 100 is injected into the heavy ladle iron ladle 1. When the heavy ladle iron ladle 1 is moved, the casting slag and sticky slag on the surface of the heavy ladle iron ladle 1 are impacted by the flame of the clustered jet oxygen lance 2 at intervals, the sticky slag is heated and melted, and the casting slag in the heavy ladle iron ladle is continuously stirred and churned. At the same time, the CO gas and O2 overflowing from the casting slag are ignited by the flame of the clustered jet oxygen lance 2 for combustion; the interval time of the impact of the clustered jet oxygen lance 2 is 5 to 10 minutes, and the time of each impact is 3 to 5 minutes; the smoke generated after combustion is absorbed and treated by the dust hood 3 and then discharged;
[0041] Repeat the above operation until the heavy ladle 1 has completed receiving the casting slag;
[0042] 3) Return the heavy iron ladle 1 after receiving the casting slag to production and utilization.
[0043] Example 2
[0044] A method for preventing casting slag from sticking to a heavy-clad iron ladle by using a clustered jet oxygen lance comprises the following steps:
[0045] 1) After the molten iron is filled into the ladle, it is ready for use. The amount of molten iron filled is 10% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle;
[0046] 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle. When sticky slag is generated at the contact between the inner wall of the heavy ladle iron ladle and the surface casting slag, the surface casting slag and sticky slag are impacted by the flame of the clustered jet oxygen gun at intervals, the sticky slag is heated and melted, and the casting slag in the heavy ladle iron ladle is continuously stirred and tumbled. At the same time, the CO gas and O2 overflowing from the casting slag are ignited by the flame of the clustered jet oxygen gun for combustion;
[0047] Repeat the above operation until the heavy ladle completes receiving the casting slag;
[0048] 3) Return the heavy ladle that receives the casting slag to production.
[0049] Example 3
[0050] A method for preventing casting slag from sticking to a heavy-clad iron ladle by using a clustered jet oxygen lance comprises the following steps:
[0051] 1) After the molten iron is filled into the ladle, it is ready for use. The amount of molten iron filled is 10% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle;
[0052] 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle, and the surface of the casting slag is impacted by a clustered jet oxygen lance at intervals, so that the casting slag in the heavy ladle iron ladle is continuously stirred and tumbled, and at the same time, the CO gas and O2 overflowing from the casting slag are ignited by the flame of the clustered jet oxygen lance for combustion; the interval time of the clustered jet oxygen lance impact is 5 to 10 minutes, and the time of each impact is 3 to 5 minutes;
[0053] Repeat the above operation until the heavy ladle completes receiving the casting slag;
[0054] 3) Return the heavy ladle that receives the casting slag to production for utilization.
Claims
1. A method for preventing casting slag from sticking to a heavy iron ladle by using a clustered jet oxygen lance. Its characteristics are: The steps include: 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled is 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle; 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle. When the heavy ladle iron ladle is moved, the surface casting slag in the heavy ladle iron ladle does not shake, or sticky slag is generated at the contact between the inner wall of the heavy ladle iron ladle and the surface casting slag, the surface casting slag and sticky slag are impacted with a concentrated jet oxygen gun flame, the sticky slag is heated and melted, and the casting slag in the heavy ladle iron ladle is continuously stirred and churned; Alternatively, after the casting slag in the ladle is injected into the heavy ladle iron ladle, a cluster jet oxygen lance is immediately used to impact the surface of the casting slag; At the same time, CO gas and O 2 The combustion is ignited by the flame of the clustered jet oxygen lance; Repeat the above operation until the heavy ladle completes receiving the casting slag; 3) Return the heavy ladle that receives the casting slag to production.
2. The method according to claim 1, Its characteristics are: In step 2), a concentrated jet oxygen lance is used to continuously or intermittently impact the casting slag and sticky slag on the surface.
3. The method according to claim 1, Its characteristics are: In step 2), during the impact process, the distance between the concentrated jet oxygen lance and the casting slag does not exceed 1.2 m.