Titanium-based electrode stability testing method based on actual working conditions

By determining the composition and dissolution process of the active oxide on the surface of the electrode in the DSA electrode stability test, and evaluating its service life under actual operating conditions, the difference in roughness and failure mechanism of the DSA electrode stability prediction method in the prior art is solved. The problem has achieved more accurate life prediction and operating rules that are closer to actual working conditions.

CN119087099APending Publication Date: 2024-12-06XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411384869.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing DSA electrode stability prediction methods cannot accurately reflect the service life of the electrode under actual operating conditions through enhanced life tests, and the failure mechanism is different from the actual situation, so the actual service life of the titanium-based electrode cannot be effectively predicted.

Method used

The service life of the electrode is evaluated by determining the composition of the active oxide on the surface of the electrode, the molar rate of the active metal dissolution, the coating mass and the failure coefficient.

Benefits of technology

This method can more accurately predict the service life of the DSA electrode, avoiding the roughness and uncertainty of the enhanced life test, and the results are closer to the operating rules under actual operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087099A_ABST
    Figure CN119087099A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrode stability testing, and relates to a titanium-based electrode stability testing method based on an actual working condition, which comprises the following steps: step 1, determining the specific composition of a surface active oxide of a titanium-based metal oxide DSA electrode to be tested, and analyzing the dissolution process of the surface active oxide under the actual working condition; step 2, testing the molar rate v of active metal dissolution of the electrode under actual working conditions; 3, determining the mass mtotal of the active oxide coating on the surface layer of the electrode; step 4, determining the failure coefficient eta% of the electrode, that is, when eta% of the coating is dissolved, the electrode fails; according to the titanium-based electrode stability evaluation test scheme provided by the invention, the service life prediction of the electrode is more accurate, and the method is closer to the operation rule of the DSA electrode under the actual working condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode stability testing, and relates to a titanium-based electrode stability testing method based on actual working conditions. Background Art

[0002] The stability and catalytic performance of electrodes have always been important contents in the research of electrochemical water treatment technology. The stability of titanium-based metal oxide (DSA) electrodes is an important factor that determines their usability. Under normal conditions of use, the performance of DSA electrodes will remain unchanged for a long time, which is not conducive to judging the stability of the electrode. Therefore, the stability of the electrode is often reflected by the enhanced test life value under more harsh conditions. The so-called enhanced life test generally uses the time for the electrode potential to rise to a certain artificially specified value under constant current to determine whether the oxide layer on the surface of the electrode has failed. The DSA electrode stability prediction method currently used by academia and industry relies on the enhanced life formula:

[0003]

[0004] Among them, T 实际 is the actual predicted service life of the electrode (h); T 强化 is the strengthening life time of the electrode (h); i 强化 is the current density value of the electrode strengthening life test (A / cm 2 );i 实际 is the current density of the electrode under actual working conditions (A / cm 2 );n reflects the relative influence of electrolyte on electrode life, which is generally 1.4~2.0.

[0005] However, the DSA electrode stability prediction method in the prior art has the following disadvantages:

[0006] At present, the failure reasons of DSA electrodes can be summarized into the following three situations: ① The dissolution of metal oxides on the electrode surface (i.e., slow chemical dissolution); ② The diffusion of new ecological oxygen into the matrix causes the passivation of the titanium matrix (i.e., the formation of non-conductive TiO2); ③ The oxygen generated in the anode micro-area impacts the surface active coating, causing the mechanical shedding of the active layer. In traditional enhanced life tests, the electrodes are placed in a strong acid and extreme current density environment. Therefore, the causes of electrode failure are often mainly due to situations ② and ③. Figure 1 As shown, at 0.5A / cm 2 Under the enhanced life test conditions of 1 mol / L H2SO4, the active layer on the electrode surface showed obvious block shedding (Case ③). Figure 2As shown in the figure, during the strengthening test, the voltage-time curve of the DSA electrode showed a typical rapid deactivation stage after 83 hours, which indicated that the titanium matrix was oxidized to generate non-conductive TiO2, causing the cell voltage to rise rapidly (case ②).

[0007] The electrolyte was tap water with a small amount of sodium sulfate added (conductivity was 3.87 mS / cm), and the current density was controlled at 20 mA / cm 2 To simulate actual working conditions. Figure 3 As shown in the figure, the condition of the active layer on the electrode surface is similar in each stage, and no obvious block shedding occurs. Figure 4 The XRD shows that the types of electrode phases at each stage are not much different, all composed of RuO2, IrO2 and a small amount of Ti, and the peak intensity has no obvious change. This shows that the failure mechanism of the Ti / Ru-Ir electrode under actual working conditions is dominated by the first case, that is, the slow chemical dissolution of the metal oxide on the surface of the electrode. This is completely different from the electrode failure mechanism of the traditional enhanced life test. In addition, the current value i in the above formula can only reflect the "input amount" of the entire electrolytic system. Although the n value can correct the difference in enhanced life caused by different electrolyte environments to a certain extent, the n value has a very large randomness, and there is currently no specific limit on the n value in the industry.

[0008] Therefore, the actual service life of the DSA electrode cannot be simply predicted by the results of the enhanced life test. A titanium-based electrode stability test method that combines the DSA electrode under actual working conditions is needed to solve the above technical problems. Summary of the invention

[0009] The technical solution adopted by the present invention to solve the technical problem is: a titanium-based electrode stability testing method based on actual working conditions, the method comprising the following steps:

[0010] Step 1, determine the specific composition of the active oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested, and analyze its dissolution process under actual working conditions;

[0011] Step 2, testing the molar rate v of active metal dissolution of the electrode under actual working conditions;

[0012] Step 3: Determine the mass m of the active oxide coating on the electrode surface total ;

[0013] Step 4: Determine the failure coefficient η% of the electrode, that is, the electrode fails when η% of the coating is dissolved.

[0014] Preferably, in step 1, the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested includes: a single metal oxide MO x 、Multinary metal oxide PNy O x ; Wherein, M, P, N represent metal elements respectively, O represents oxygen element, and x and y represent numerical subscripts of the molecular formula respectively.

[0015] More preferably, in step 1, when the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested is a single metal oxide MO x The dissolution process is:

[0016] MO x + 2x H + → M 2x+ + x H2O (1).

[0017] More preferably, in step 2, the molar rate v of active metal dissolution is:

[0018]

[0019] In formula (2), M 金 is the relative molecular mass of metal M (g / mol), V is the volume of electrolyte (L), m M is the mass of dissolved metal ion M (mg), C M is the concentration of dissolved metal ions M, and t is the electrolysis time (h).

[0020] More preferably, in step 2, the concentration of metal ions dissolved in the electrolyte is tested using inductively coupled plasma-optical emission spectroscopy (ICP-OES).

[0021] More preferably, in step 4, the use time of the titanium matrix metal oxide DSA electrode to be tested is:

[0022]

[0023] In formula (3), n 金 is the molar amount of metal in the electrode coating (mol), M MOx Metal oxide MO x Relative molecular mass (g / mol).

[0024] More preferably, in step 1, when the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested is a multi-metal oxide PN y O x The dissolution process is:

[0025] PN y O x + 2x H + → P +(2x-zy) +yN +z+x H2O (4).

[0026] More preferably, in step 2, the molar rate v of active metal dissolution is:

[0027]

[0028]

[0029] In formula (5) and (6), v P and v N are the molar rates of metal P and metal N dissolution (mol / h), V is the volume of electrolyte (L), n P and n N are the molar masses (mol) of metal ions P and N, respectively. P and M N are the relative molecular masses (g / mol) of metal P and metal N, respectively. P and C N are the concentrations of metal P and metal N (mg / L), and t is the electrolysis time (h).

[0030] More preferably, in step 4, when P and N are dissolved synchronously at equal molar rates, the use time of the titanium matrix metal oxide DSA electrode to be tested is:

[0031]

[0032] In formula (7), M PNyOx PN is a metal oxide y O x Relative molecular mass (g / mol).

[0033] Preferably, in step 4, when P and N dissolve at different molar rates, the metal that dissolves faster is used as the main metal, and the use time of the titanium matrix metal oxide DSA electrode to be tested is:

[0034]

[0035] In formula (8), n 主 is the molar amount of the main metal in the electrode coating (mol), M 主 is the relative molecular mass of the main metal in the electrode coating (g / mol), M PNyOx is the relative molecular mass of the main metal oxide (g / mol).

[0036] The beneficial effects of the present invention are:

[0037] The actual life prediction method of the DSA electrode proposed in the present invention is based on the slow failure process of the DSA electrode under actual working conditions, and is supported by abundant theoretical and experimental results, avoiding the roughness and uncertainty of the existing enhanced life test methods. In the embodiment of the present invention, the Ti / Ru-Ir electrode is used as one of the typical DSA electrodes, and its service life under actual working conditions is tested to be about 11000h; the service life of the Ti / Ru-Ir electrode predicted by the traditional enhanced life test scheme is about 8879h; the service life of the Ti / Ru-Ir electrode predicted by the present invention is about 10331h; therefore, the DSA electrode stability evaluation test scheme proposed in the present invention is more accurate in predicting the life of the DSA electrode, and the method described in the present invention is closer to the operating law of the DSA electrode under actual working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a SEM comparison of the Ti / Ir-Ru electrode of the prior art before and after the enhanced life test; (a) before the test, (b) after the test;

[0039] Figure 2 It is a voltage-time curve diagram during the Ti / Ir-Ru electrode strengthening test process in the prior art;

[0040] Figure 3 These are SEM comparison images of the Ti / Ir-Ru electrode of the prior art at various stages of actual working condition testing; (a) 200h, (b) 400h, (c) 600h, (d) 800h, (e) 1000h, (f) 1200h;

[0041] Figure 4 This is the XRD comparison diagram of the existing Ti / Ir-Ru electrode at each stage of the actual working condition test;

[0042] Figure 5 It is a schematic diagram of a titanium-based electrode stability testing method based on actual working conditions of the present invention. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the relevant technologies in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] refer to Figures 1 to 5 The present invention provides a titanium-based electrode stability evaluation test scheme based on actual working conditions, including:

[0045] 1. Determine the specific composition of the active oxides on the surface of the DSA electrode to be tested and analyze its dissolution process under actual working conditions.

[0046] 2. Test the molar rate v (mol / h) of active metal dissolution of the electrode under actual working conditions.

[0047] 3. Determine the mass m of the active oxide coating on the surface of the DSA electrode to be tested total (g).

[0048] 4. Clarify the failure coefficient η% of the electrode, that is, the electrode fails when η% of the coating is dissolved.

[0049] Test plan 1:

[0050] According to step 1, when the active metal oxide on the surface of the DSA electrode is a single metal oxide (MO x ), its dissolution process under actual working conditions is:

[0051] MO x + 2x H + → M 2x+ + x H2O (1)

[0052] According to step 2, under actual working conditions, the electrode is first electrolyzed in an electrolyte with a volume of V (L) for a period of time t (h), and preferably, the concentration C of the metal ion M dissolved in the electrolyte is tested by ICP-OES. M (mg / L). Then the mass of M is m M (mg) is:

[0053] m M =V×C M

[0054] The molar rate v (mol / h) of dissolution of the DSA electrode during its entire life cycle is:

[0055]

[0056] Among them, M 金 is the relative molecular mass of metal M (g / mol).

[0057] According to step 3, the mass m of the active oxide coating on the surface of the DSA electrode to be tested is determined. total (g).

[0058] According to step 4, the failure coefficient η% of the DSA electrode to be tested is determined. The η% value will change and fluctuate according to individual factors such as the actual electrode formula and preparation process of each electrode manufacturer. In particular, there are multiple oxide layer protrusions on the surface of the electrode, which will cause the dissolution process to be non-uniform. At this time, the η% value should be estimated based on the situation of the most concave part of the electrode surface.

[0059] The molar amount of metal in the titanium electrode coating is n 金 (mol) is:

[0060]

[0061] Among them, M MOx Metal oxide MO x Relative molecular mass (g / mol).

[0062] The titanium electrode (MO x ) The usage time (h) under actual working conditions is:

[0063]

[0064] Test plan 2:

[0065] According to step 1, when the active metal oxide on the surface of the DSA electrode is a multi-metal oxide (PN y O x ), its dissolution process under actual working conditions is (assuming the valence state of metal N is +z, then the valence state of metal P is +(2x-zy)):

[0066] PN y O x + 2x H + → P +(2x-zy) +yN +z +x H2O (4)

[0067] According to step 2, under actual working conditions, the electrode is first electrolyzed in an electrolyte with a volume of V (L) for a period of time t (h), and then the concentrations of P and N in the electrolyte are measured by ICP. P and C N (mg / L). Then the mass of dissolved metal ions P and N is m P and m N (mg) are:

[0068] m P =V×C P

[0069] m N =V×C N

[0070] The molar mass n of the dissolved metal ions P and N P and n N (mol) are:

[0071]

[0072] Among them, M P and M N are the relative molecular masses (g / mol) of metal P and metal N respectively.

[0073] The molar rate of P and N dissolution in the DSA electrode during its entire life cycle is v P and v N (mol / h) are:

[0074]

[0075] According to step 3, the mass m of the active oxide coating on the surface of the DSA electrode to be tested is determined. total (g).

[0076] According to step 4, the failure coefficient η% of the DSA electrode to be tested is determined. At this time, there are the following two situations:

[0077] 1) P and N dissolve synchronously at equal molar rates, that is:

[0078]

[0079] Then we can arbitrarily select metal P or N to evaluate the titanium electrode (PN y O x ) can be used for the actual working time (h). The molar mass n of metal P and N in the metal oxide coating P and n N (mol) are:

[0080]

[0081] Among them, M PNyOx PN is a metal oxide y O x Relative molecular mass (g / mol).

[0082] Then the electrode (PN y O x ) The usage time (h) under actual working conditions is:

[0083]

[0084] 2) P and N dissolve at different molar rates, that is:

[0085] (P metal dissolves faster) or (N metal dissolves faster)

[0086] The metal that dissolves faster is used as the main metal. y O x )Use under actual working conditions

[0087] The time is calculated using the single metal oxide titanium electrode method in formula (8):

[0088]

[0089] In formula (8), n 主 is the molar amount of the main metal in the electrode coating, M 主 is the relative molecular mass of the main metal in the electrode coating, M PNyOx Relative molecular mass of the main metal oxide.

[0090] Example

[0091] Embodiment 1:

[0092] (1) Prepare a 1 mol / L sulfuric acid solution with deionized water. Use the "two negatives and one positive" method, with a 2×2 cm Ti / Ru-Ir electrode (the mass ratio of RuO2 and IrO2 in the coating is 1:1) as the anode and two titanium electrodes of the same size as the cathode. The cathode and the anode are aligned and placed parallel to each other with a spacing of 1.5 cm. Immerse the electrode in the above sulfuric acid solution. Control the current density to 0.5 A / cm 2 When the cell voltage reaches 10 V, the electrode is judged to be inactivated.

[0093] (2) When the cell voltage reaches 10 V, the Ti / Ru-Ir electrode in this embodiment operates for 98 h. The life of the Ti / Ru-Ir electrode under actual working conditions is estimated. The current density i under actual working conditions in this embodiment is 实际 Take 0.02A / cm 2 , nxy value is 1.4. Then the actual life of the electrode is calculated to be approximately:

[0094]

[0095] Embodiment 2:

[0096] (1) Sodium sulfate was used as the electrolyte, and tap water was used to prepare a simulated electrolyte with a volume of 1L and a conductivity of 3.87mS / cm under actual working conditions. The "two negatives and one positive" method was adopted, with a 2×2cm Ti / Ru-Ir electrode (the mass ratio of RuO2 and IrO2 in the coating was 1:1) as the anode and two titanium electrodes of the same size as the cathode. The cathode and the anode were aligned and placed in parallel with a spacing of 1.5cm. The electrode sheet was immersed in the above-mentioned simulated electrolyte. The current density was controlled to be 0.02A / cm 2 , and the power is continuously applied, the initial cell voltage of the electrode is 6.8V.

[0097] (2) During the test, the electrochemical properties of the electrode were monitored every 400 h, and deionized water was added in a timely manner to ensure that the electrode was always immersed in the electrolyte.

[0098] (3) When the electrochemical properties of the Ti / Ru-Ir electrode in the example are similar to those of the electrode tested in Example 1, that is, the oxygen evolution overpotential decreases from 1.44 V to 1.1 V, and the electrode film resistance decreases from 0.38 Ω·cm to 13 Ω·cm, the electrode is considered to be inactivated.

[0099] (4) In this embodiment, the Ti / Ru-Ir electrode has been in operation for about 11,000 hours when the electrochemical parameters shown in (3) are reached, that is, the service life of the electrode under actual working conditions is about 11,000 hours. At this time, the electrode before and after operation is weighed by an electronic balance, and it is found that the mass of the Ti / Ru-Ir electrode in this embodiment is reduced from 3104.5 mg to 2177.7 mg, and the molar mass is reduced from 0.0087 mol to 0.0061 mol, that is, about 70% of the active coating is dissolved during the electrolysis process.

[0100] Embodiment 3:

[0101] (1) Sodium sulfate was used as the electrolyte, and tap water was used to prepare a simulated electrolyte with a volume of 1L and a conductivity of 3.87mS / cm under actual working conditions. The "two negatives and one positive" method was adopted, with a 2×2cm Ti / Ru-Ir electrode (the mass ratio of RuO2 and IrO2 in the coating was 1:1) as the anode and two titanium electrodes of the same size as the cathode. The cathode and the anode were aligned and placed in parallel with a spacing of 1.5cm. The electrode sheet was immersed in the above-mentioned simulated electrolyte. The current density was controlled to be 0.02A / cm 2 , power is applied for 10 hours, and preferably, the amount of Ru and Ir metal dissolved in the solution is determined by ICP-OES.

[0102] (2) In this embodiment, the active metal oxide on the surface of the Ti / Ru-Ir electrode is a multi-metal oxide. Since the mass ratio of RuO2 and IrO2 in the coating is 1:1, according to the relative atomic masses M of the two metals,Ru =101 g / mol and M Ir =192 g / mol, the metal compound can be recorded as RuIr 1.9 O 5.8 , its dissolution process under actual working conditions is:

[0103] R 1.9 O 5.8 +11.6H + →Ru +4 +1.9Ir +4 +5.8H2O

[0104] (3) ICP-OES was used to test the Ru content in the electrolyte after 10 hours of reaction. +4 and Ir +4 The concentration of C Ru and C Ir They are 0.001917mg / L and 0.001928mg / L respectively. From the above formula, we can get the dissolved metal ion Ru +4 and Ir +4 The mass m Ru and m Ir (mg) are:

[0105] m Ru =V×C Ru =0.001917mg

[0106] m Ir =V×C Ir =0.001928mg

[0107] (4) It can be seen that the molar mass n of the dissolved metal ions P and N Ru and n Ir (mol) are:

[0108]

[0109]

[0110] (5) In this embodiment, the Ti / Ru-Ir electrode has a Ru +4 and Ir +4 Molar rate of dissolution v Ru and v Ir (mol / h) are:

[0111]

[0112]

[0113] (5) In this embodiment, the total mass of the active oxide coating on the surface of the Ti / Ru-Ir electrode is 0.01 g. As shown in Example 2, the failure coefficient η% of the electrode is 70%. According to the above formula, Ru +4 and Ir +4 Different molar rates of dissolution, and Ru +4 The dissolution rate is faster. That is:

[0114]

[0115] The faster dissolving Ru +4 As the main metal, the service life of the Ti / Ru-Ir electrode in this embodiment under actual working conditions is calculated using the calculation method of the single metal oxide titanium electrode in the formula.

[0116] (6) In this embodiment, the service life (h) of the Ti / Ru-Ir electrode under actual working conditions is:

[0117]

[0118] In summary, the titanium-based electrode stability evaluation test method proposed in the present invention is more accurate in predicting the life of the electrode, and the method described in the present invention is closer to the operating law of the DSA electrode under actual working conditions. Therefore, the present invention has broad application prospects in the field of titanium-based electrode stability testing.

[0119] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A titanium-based electrode stability test method based on actual working conditions, characterized in that: The algorithm comprises the following steps: Step 1, determine the specific composition of the active oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested, and analyze its dissolution process under actual working conditions; Step 2, testing the molar rate v of active metal dissolution of the electrode under actual working conditions; Step 3: Determine the mass m of the active oxide coating on the electrode surface total ; Step 4: Determine the failure coefficient η% of the electrode, that is, the electrode fails when η% of the coating is dissolved.

2. A titanium-based electrode stability testing method based on actual working conditions according to claim 1, characterized in that: In the step 1, the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested includes: a single metal oxide MO x 、Multinary metal oxide PN y O x ; Wherein, M, P, N represent metal elements respectively, O represents oxygen element, and x and y represent numerical subscripts of the molecular formula respectively.

3. A titanium-based electrode stability testing method based on actual working conditions according to claim 2, characterized in that: In step 1, when the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested is a single metal oxide MO x The dissolution process is: MO x + 2x H + → M 2x+ + x H2O (1)。 4. A titanium-based electrode stability testing method based on actual working conditions according to claim 3, characterized in that: In step 2, the molar rate v of active metal dissolution is: In formula (2), M 金 is the relative molecular mass of metal M, V is the volume of electrolyte, m M is the mass of dissolved metal ions M, C M is the concentration of dissolved metal ions M, and t is the electrolysis time.

5. A titanium-based electrode stability testing method based on actual working conditions according to claim 4, characterized in that: In the step 2, the concentration of metal ions dissolved in the electrolyte is tested by inductively coupled plasma-optical emission spectroscopy (ICP-OES).

6. A titanium-based electrode stability testing method based on actual working conditions according to claim 4, characterized in that: In step 4, the use time of the titanium matrix metal oxide DSA electrode to be tested is: In formula (3), n 金 is the molar amount of metal in the electrode coating, M MOx Metal oxide MO x The relative molecular mass.

7. A titanium-based electrode stability testing method based on actual working conditions according to claim 2, characterized in that: In step 1, when the active metal oxide on the surface of the titanium matrix metal oxide DSA electrode to be tested is a multi-metal oxide PN y O x The dissolution process is: PN y Oh x + 2x H + → P +(2x-zy) + yN +z +x H2O (4)。 8. A titanium-based electrode stability testing method based on actual working conditions according to claim 7, characterized in that: In step 2, the molar rate v of active metal dissolution is: In formula (5) and formula (6), v P and v N are the molar rates of dissolution of metal P and metal N, respectively, V is the volume of electrolyte, n P and n N are the molar masses of metal ions P and N, respectively, P and M N are the relative molecular masses of metal P and metal N, respectively. P and C N are the concentrations of metal P and metal N respectively, and t is the electrolysis time.

9. A titanium-based electrode stability testing method based on actual working conditions according to claim 8, characterized in that: In step 4, when P and N are dissolved synchronously at equal molar rates, the use time of the titanium matrix metal oxide DSA electrode to be tested is: In formula (7), M PNyOx PN is a metal oxide y O x The relative molecular mass.

10. A titanium-based electrode stability testing method based on actual working conditions according to claim 8, characterized in that: In step 4, when P and N are dissolved at different molar rates, the metal that dissolves faster is used as the main metal, and the use time of the titanium matrix metal oxide DSA electrode to be tested is: In formula (8), n 主 is the molar amount of the main metal in the electrode coating, M 主 is the relative molecular mass of the main metal in the electrode coating, M PNyOx Relative molecular mass of the main metal oxide.