Preparation and application of anti-reverse pole material with core-shell structure

By performing porous carbon wrapping and ball milling on iridium oxide nanoparticles, the dispersion and settlement problems in fuel cells are solved, the anti-reverse performance and stability of the fuel cells are improved, and the homogeneity and reliability.

CN119133468APending Publication Date: 2024-12-13ANHUI TOMORROW HYDROGEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981589.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-12-13

AI Technical Summary

Technical Problem

There are dispersion problems in the preparation process of iridium oxide nanoparticles in existing fuel cells, which affect the uniformity and performance of MEA, and are prone to settlement under reverse polar conditions, affecting the stability and durability of the battery.

Method used

The iridium oxide nanoparticles are treated with porous carbon encapsulation. Through ball milling and vibration grinding, the particle size and dispersion of the nanoparticles are controlled to form a more stable porous carbon encapsulated iridium oxide nanoparticles, improve their dispersion state in the slurry, and The fuel cell membrane electrode was obtained by ultrasonic spraying and hot pressing.

Benefits of technology

The dispersion state of nano iridium oxide is significantly improved, the settlement phenomenon is reduced, the stability and anti-reverse performance of the catalyst are improved, the durability and efficiency of the fuel cell are improved, the production process is simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119133468A_ABST
    Figure CN119133468A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of an anti-reverse electrode material with a core-shell structure, and relates to the technical field of proton exchange membrane fuel cells. Comprising the following steps: S1, preparing materials; s2, preparing an anti-reverse pole material; s3, preparing slurry; s4, manufacturing a membrane electrode; wherein the material preparation comprises the following steps: nano iridium oxide with the average particle size of 5-20 nm and the purity of more than or equal to 99.9%; the carbon source adopts one or more of glucose, cane sugar and starch, and the purity is greater than or equal to 99.5%. According to the preparation method, nano iridium oxide is subjected to porous carbon wrapping treatment, so that the dispersion state of nano iridium oxide in slurry is remarkably improved; the nano particles are distributed more uniformly and can play a better role in a catalytic layer of the fuel cell; the coated nano iridium oxide shows better stability, so that the occurrence of a sedimentation phenomenon is reduced; in the preparation process, the loss of the catalyst is less, and the consistency and reliability of a final product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of proton exchange membrane fuel cells, and in particular to the preparation and application of a core-shell structure anti-reverse pole material. Background Art

[0002] With the transformation of the global energy structure and the improvement of environmental protection awareness, the research and application of clean energy technology has received widespread attention. Fuel cells, as an efficient energy conversion device that directly converts chemical energy into electrical energy, play an important role in the field of clean energy due to their high energy efficiency and low emissions. The core component of fuel cells: membrane electrode assembly (MEA), composed of a catalyst layer, a proton exchange membrane and a gas diffusion layer, is the key part of realizing electrochemical reactions.

[0003] However, in actual operation, fuel cells may encounter the so-called "reverse polarity" phenomenon, that is, due to insufficient hydrogen supply or other reasons, the anode potential abnormally rises and exceeds the cathode potential. Reverse polarity not only leads to reverse electrolysis of water, but also may cause corrosion of the carbon carrier, thereby destroying the catalyst layer structure, reducing the electrochemical active area, affecting the performance and life of the MEA, and in severe cases even causing complete damage to the battery.

[0004] In order to improve the anti-reverse polarity of fuel cells, researchers have developed a variety of strategies, one of which is to add anti-reverse polarity elements to MEA. Iridium oxide (IrO2) is considered to be an effective anti-reverse polarity element due to its high conductivity, chemical stability and catalytic activity. Iridium oxide can catalyze the oxidation reaction of water under reverse polarity conditions, reduce the occurrence of carbon corrosion, and thus improve the stability and durability of fuel cells.

[0005] However, there are difficulties in dispersing iridium oxide nanoparticles when preparing MEA slurry. Due to their high surface energy, nanoparticles are easy to agglomerate, and after high-temperature treatment, iridium oxide nanoparticles have few surface groups, especially in thin slurries, and are prone to sedimentation, which affects the uniformity and performance of MEA.

[0006] After searching, the application scheme of Chinese patent application No. 202210651211.6 discloses an anti-reverse polarity material, an anti-reverse polarity slurry, and a preparation method and application thereof. The preparation method of the anti-reverse polarity material comprises the following steps: refluxing, drying and calcining the mixed solution to obtain the anti-reverse polarity material; the mixed solution comprises an anti-reverse polarity active precursor and a stabilizer; the anti-reverse polarity active precursor comprises a water-soluble salt of M, and M comprises any one or a combination of at least two of ruthenium, cobalt, manganese, nickel or tin; the stabilizer comprises a metal oxide. The products obtained by the preparation method in the above patent are still insufficient in terms of anti-reverse polarity performance and stability. Summary of the invention

[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a preparation and application of a core-shell structure anti-reverse polarity material.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for preparing a core-shell structure anti-reversal material comprises the following steps:

[0010] S1: Material preparation;

[0011] S2: Preparation of anti-reverse polarity materials;

[0012] S3: slurry preparation;

[0013] S4: membrane electrode fabrication;

[0014] The material preparation includes:

[0015] Nano-iridium oxide: average particle size 5-20nm, purity ≥99.9%;

[0016] Carbon source: one or more of glucose, sucrose and starch, with a purity of ≥99.5%;

[0017] Wherein, in said S2, the preparation of the anti-reverse electrode material specifically comprises the following steps:

[0018] S21: Mixing ratio: mixing iridium oxide and carbon source in a mass ratio of 2:1 to 5:1;

[0019] S22: Ball milling equipment: Choose a ball mill with circulating cooling water, and the ball mill tank is made of polytetrafluoroethylene;

[0020] S23: low-speed ball milling;

[0021] S24: high-speed ball milling;

[0022] S25: low temperature dehydration: heat treating the mixture at 250-350°C for 12-24 hours under an inert gas atmosphere;

[0023] S26: grinding process.

[0024] Preferably: in S23, the ball milling speed of the low-speed ball mill is set to 100-200 RPM for 30 minutes, and the temperature of the ball mill is controlled to be ≤20° C. using a circulating cold water system;

[0025] In S24, the ball milling speed is increased to 800-1000 RPM for 4-10 hours, and the temperature of the ball mill is controlled to be ≤200° C. using a circulating water system.

[0026] Preferably, in S26, the specific method of grinding is:

[0027] The carbonized product was placed in a vibration mill and ZrO 2 As ball milling media, set the ball-to-material ratio to 15:1 to 20:1, adjust the vibration frequency to 15-30 Hz, adjust the amplitude to 1-5 mm, set the grinding time to 1-10 hours, and control the temperature within 30°C.

[0028] Preferably, in said S26, during the grinding process:

[0029] The particle size is controlled by laser particle size analysis, D50 is less than 0.2 micron, and D90 is less than 1 micron; and porous carbon-wrapped iridium oxide nanoparticles are obtained.

[0030] Preferably: in S3, the slurry preparation specifically includes the preparation of cathode slurry and the preparation of anode slurry, wherein the preparation of cathode slurry includes the following steps:

[0031] Cathode slurry: using ionomer resin DuPont D2020, Pt / C catalyst with a platinum content of 50%, and a solvent system of water and isopropanol mixed in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the catalyst carbon carrier to 0.8; stirring the mixed slurry, and then dispersing it.

[0032] Preferably: in the preparation of the cathode slurry, the stirring and dispersion of the mixed slurry are specifically as follows:

[0033] The mixed slurry was stirred with a high-speed stirrer at a speed of 10,000 rpm for 30 minutes to ensure adequate dispersion of the catalyst, followed by ultrasonic dispersion at 300 W for 30 minutes. The temperature did not exceed 10° C. during the entire slurry preparation process.

[0034] Preferably, the preparation of the anode slurry comprises the following steps:

[0035] Anode slurry: using ionomer resin DuPont D2020 (solid content 20%), Pt / C catalyst with a platinum content of 50%, and porous carbon-wrapped iridium oxide nanoparticles prepared in the above steps, the solvent system is a solvent mixed with water and isopropanol in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the carbon carrier of the Pt / C catalyst (IC ratio) to 0.8; using a high-speed stirrer to stir the mixed slurry, the stirring speed is set to 10000rpm, and it lasts for 30 minutes to ensure that the catalyst is fully dispersed, and then 300W ultrasonic dispersion is performed for 30 minutes. The temperature does not exceed 10°C during the entire slurry preparation process.

[0036] Preferably, in the preparation of the anode slurry, the mass ratio of Pt to Ir in the catalyst slurry is controlled within a range of 30:1 to 5:1.

[0037] Preferably, in S4, the membrane electrode manufacturing specifically includes the following steps:

[0038] The prepared slurry was ultrasonically sprayed, and the nozzle movement speed and discharge speed were adjusted to control the anode platinum loading to 0.1 mg / cm 2 , the cathode platinum loading is 0.35 mg / cm 2 .

[0039] Preferably: in S4, during the ultrasonic spraying process, the temperature of the proton membrane carrier is 85°C; after the anode and cathode slurry spraying is completed, a 220μm gas diffusion layer is attached to both sides of the above-mentioned catalyst membrane, loaded into the mold of a hot press, and hot-pressed at 140°C and 3MPa pressure for 2 minutes to obtain a fuel cell membrane electrode.

[0040] The beneficial effects of the present invention are:

[0041] 1. The present invention significantly improves the dispersion state of nano-iridium oxide in the slurry by performing porous carbon encapsulation treatment on the nano-iridium oxide; the nano-particles are more evenly distributed and can play a better role in the catalytic layer of the fuel cell; the encapsulated nano-iridium oxide shows better stability and reduces the occurrence of sedimentation; during the preparation process, the catalyst is less lost, which helps to improve the consistency and reliability of the final product.

[0042] 2. The fuel cell membrane electrode of the present invention shows a lower voltage decay rate, which indicates that the treated catalyst has better anti-reverse polarity performance; it is crucial to improve the durability and efficiency of the fuel cell; since the encapsulated nanoparticles have better dispersion, higher homogeneity and stability can be achieved during the slurry preparation process; the slurry processing steps are simplified, the production cost is reduced, and the product quality is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A flow chart for preparing a core-shell structure anti-reverse electrode material proposed by the present invention;

[0044] Figure 2 TEM images of iridium oxide nanoparticles before and after porous carbon encapsulation in the preparation of a core-shell structure anti-reverse polarity material proposed in the present invention. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0046] Embodiment 1:

[0047] A preparation method of a core-shell structure anti-reversal material comprises the following steps:

[0048] S1: Material preparation;

[0049] S2: Preparation of anti-reverse polarity materials;

[0050] S3: slurry preparation;

[0051] S4: membrane electrode fabrication;

[0052] The material preparation includes:

[0053] Nano-iridium oxide (IrO 2 ): average particle size 5-20nm, purity ≥99.9%;

[0054] Carbon source: Glucose, sucrose, starch can be used, purity ≥ 99.5%;

[0055] Wherein, in said S2, the preparation of the anti-reverse electrode material specifically comprises the following steps:

[0056] S21: Mixing ratio: mixing iridium oxide and carbon source in a mass ratio of 2:1 to 5:1;

[0057] S22: Ball milling equipment: Choose a ball mill with circulating cooling water, and the ball mill tank is made of polytetrafluoroethylene;

[0058] S23: low-speed ball milling;

[0059] S24: high-speed ball milling;

[0060] S25: low temperature dehydration: heat treating the mixture at 250-350°C for 12-24 hours under an inert gas atmosphere;

[0061] S26: grinding process.

[0062] Wherein, in S23, the ball milling speed of the low-speed ball milling is set to 100-200 RPM, which lasts for 30 minutes, and the temperature of the ball milling tank is controlled to be ≤20° C. using a circulating cold water system;

[0063] In S24, the ball milling speed is increased to 800-1000 RPM for 4-10 hours, and the temperature of the ball mill is controlled to be ≤200° C. using a circulating water system.

[0064] Among them, in said S26, the specific method of grinding treatment is:

[0065] The carbonized product was placed in a vibration mill and ZrO 2(particle size 1.0-1.2mm) as ball milling media, set the ball-to-material ratio to 15:1 to 20:1, adjust the vibration frequency to 15-30Hz, adjust the amplitude to 1-5mm, set the grinding time to 1-10 hours, and control the temperature within 30℃.

[0066] Wherein, in said S26, during the grinding process:

[0067] The particle size is controlled by laser particle size analysis, D50 is less than 0.2 micron, and D90 is less than 1 micron; and porous carbon-wrapped iridium oxide nanoparticles are obtained.

[0068] In S3, the slurry preparation specifically includes the preparation of cathode slurry and the preparation of anode slurry, wherein the preparation of cathode slurry includes the following steps:

[0069] Cathode slurry: using ionomer resin DuPont D2020 (solid content 20%), Pt / C catalyst with a platinum content of 50%, and a solvent system of a solvent mixed with water and isopropanol in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the catalyst carbon carrier (IC ratio) to 0.8; stirring the mixed slurry, and then dispersing it;

[0070] In the preparation of the cathode slurry, the stirring and dispersion of the mixed slurry are specifically as follows:

[0071] The mixed slurry was stirred with a high-speed stirrer at a speed of 10,000 rpm for 30 minutes to ensure adequate dispersion of the catalyst, followed by ultrasonic dispersion at 300 W for 30 minutes. The temperature did not exceed 10° C. during the entire slurry preparation process.

[0072] Wherein, the preparation of the anode slurry comprises the following steps:

[0073] Anode slurry: using ionomer resin DuPont D2020 (solid content 20%), Pt / C catalyst with a platinum content of 50%, and porous carbon-wrapped iridium oxide nanoparticles prepared in the above steps, the solvent system is a solvent mixed with water and isopropanol in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the carbon carrier of the Pt / C catalyst (IC ratio) to 0.8; using a high-speed stirrer to stir the mixed slurry, the stirring speed is set to 10000rpm, and it lasts for 30 minutes to ensure that the catalyst is fully dispersed, and then 300W ultrasonic dispersion is performed for 30 minutes. The temperature does not exceed 10°C during the entire slurry preparation process.

[0074] Wherein, in the preparation of the anode slurry, the mass ratio of Pt to Ir in the catalyst slurry is controlled in the range of 30:1 to 5:1.

[0075] Among them, in S4, the membrane electrode manufacturing specifically includes the following steps:

[0076] The prepared slurry was ultrasonically sprayed, and the nozzle movement speed and discharge speed were adjusted to control the anode platinum loading to 0.1 mg / cm 2 , the cathode platinum loading is 0.35 mg / cm 2 ;

[0077] Among them, in the S4, during the ultrasonic spraying process, the temperature of the proton membrane carrier is 85°C; after the anode and cathode slurry spraying is completed, a 220μm gas diffusion layer is attached to both sides of the above-mentioned catalyst membrane, loaded into the mold of the hot press, and hot-pressed at 140°C and 3MPa pressure for 2 minutes to obtain a fuel cell membrane electrode.

[0078] Comparative Example:

[0079] Compared with the embodiment, the comparative example does not perform any pretreatment on the nano-iridium oxide, and the remaining steps are the same.

[0080] Test method: Anti-reverse performance test: The catalysts prepared in the examples and comparative examples are prepared into the anode catalyst layer of the fuel cell, and the anti-reverse performance of the catalyst in the single cell is tested. Polarization curve tests are performed before and after the reverse polarity test, and the polarization curve at 2000mA / cm2 is recorded after the battery is reversed 20 times. 2 The voltage attenuation at .

[0081] The above examples and comparative examples investigate the effect comparison of porous carbon encapsulation treatment on nano-iridium oxide. From the example (nano-iridium oxide average particle size 10nm; carbon source selected glucose; mass ratio of iridium oxide to carbon source 4:1; low-speed ball milling speed set to 200RPM; high-speed ball milling speed set to 1000RPM, continued for 10 hours; low-temperature dehydration temperature set to 350℃, heat treatment time set to 24 hours; in the grinding step: ZrO 2 The medium particle size is 1.0-1.2 mm, the ball-to-material ratio is 20:1, the vibration frequency is 30 Hz, the amplitude is 5 mm, the grinding time is 10 hours, and the temperature is controlled within 30°C. In the slurry preparation step, the mass ratio of Pt to Ir in the anode catalyst slurry is controlled at 20:1. By comparing the TEM images of the iridium oxide nanoparticles after encapsulation and the nanoparticles before encapsulation, it can be seen that the iridium oxide nanoparticles before encapsulation are in a piled state, and the nanoparticles after encapsulation are in a better dispersed state, indicating that the surface polarity of the iridium oxide nanoparticles is enhanced after encapsulation, and it is easier to reach a stable state in the slurry.

[0082] Voltage attenuation before and after polarity reversal in the embodiment and comparative example

[0083] <![CDATA[Voltage @ 2000 mA / cm 2 > Voltage attenuation (%) Example 0.642 1.23% Comparative Example 0.545 16.15%

[0084] From the comparison of the post-reverse polarity performance in the above table, it can be seen that the attenuation voltage of the embodiment is significantly lower than that of the comparative example, indicating that the iridium oxide in the embodiment is better dispersed. The better dispersed iridium oxide can exert better anti-reverse polarity performance. In addition, better dispersion can reduce the sedimentation of iridium oxide and allow more iridium oxide to participate in the anti-reverse polarity reaction.

[0085] Changes in solid content of upper slurry in Examples and Comparative Examples

[0086] Initial slurry Leave for 10 minutes Leave for 30 minutes Example 2% 1.99% 1.98% Comparative Example 2% 1.91% 1.85%

[0087] From the changes in the solid content of the upper slurry of the embodiment and the comparative example in the above table, it can be seen that the solid content of the embodiment slurry did not change significantly during the placement process, and the solid content of the upper part of the comparative slurry continued to decrease during the placement process, indicating that there is a sedimentation phenomenon of iridium oxide, which is consistent with the conclusion obtained previously. From the above conclusions, it can be seen that by wrapping iridium oxide nanoparticles with porous carbon by the method of this patent, the dispersion state of nano-iridium oxide in the slurry can be effectively improved, thereby reducing the sedimentation of nano-iridium oxide in the slurry and improving the anti-reverse polarity performance of the membrane electrode.

[0088] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a core-shell structure anti-reversal material, It is characterized in that The steps include: S1: Material preparation; S2: Preparation of anti-reverse polarity materials; S3: slurry preparation; S4: membrane electrode fabrication; The material preparation includes: Nano-iridium oxide: average particle size 5-20nm, purity ≥99.9%; Carbon source: one or more of glucose, sucrose and starch, with a purity of ≥99.5%; Wherein, in said S2, the preparation of the anti-reverse electrode material specifically comprises the following steps: S21: Mixing ratio: mixing iridium oxide and carbon source in a mass ratio of 2:1 to 5:1; S22: Ball milling equipment: Choose a ball mill with circulating cooling water, and the ball mill tank is made of polytetrafluoroethylene; S23: low-speed ball milling; S24: high-speed ball milling; S25: low temperature dehydration: heat treating the mixture at 250-350°C for 12-24 hours under an inert gas atmosphere; S26: grinding process.

2. The method for preparing a core-shell structure anti-reversal material according to claim 1, It is characterized in that In S23, the ball milling speed of the low-speed ball mill is set to 100-200 RPM for 30 minutes, and the temperature of the ball mill is controlled to be ≤20° C. using a circulating cold water system; In S24, the ball milling speed is increased to 800-1000 RPM for 4-10 hours, and the temperature of the ball mill is controlled to be ≤200° C. using a circulating water system.

3. The method for preparing a core-shell structure anti-reversal material according to claim 2, It is characterized in that In S26, the specific method of grinding is: The carbonized product was placed in a vibration mill and ZrO 2 As ball milling media, set the ball-to-material ratio to 15:1 to 20:1, adjust the vibration frequency to 15-30 Hz, adjust the amplitude to 1-5 mm, set the grinding time to 1-10 hours, and control the temperature within 30°C.

4. The method for preparing a core-shell structure anti-reversal material according to claim 3, It is characterized in that In the S26, during the grinding process: The particle size is controlled by laser particle size analysis, D50 is less than 0.2 micron, and D90 is less than 1 micron; and porous carbon-wrapped iridium oxide nanoparticles are obtained.

5. The method for preparing a core-shell structure anti-reversal material according to claim 2, It is characterized in that In S3, the slurry preparation specifically includes the preparation of cathode slurry and the preparation of anode slurry, wherein the preparation of cathode slurry includes the following steps: Cathode slurry: using ionomer resin DuPont D2020, Pt / C catalyst with a platinum content of 50%, and a solvent system of water and isopropanol mixed in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the catalyst carbon carrier to 0.8; stirring the mixed slurry, and then dispersing it.

6. The method for preparing a core-shell structure anti-reversal material according to claim 5, It is characterized in that In the preparation of the cathode slurry, the stirring and dispersion of the mixed slurry are specifically as follows: The mixed slurry was stirred with a high-speed stirrer at a speed of 10,000 rpm for 30 minutes to ensure adequate dispersion of the catalyst, followed by ultrasonic dispersion at 300 W for 30 minutes. The temperature did not exceed 10° C. during the entire slurry preparation process.

7. The method for preparing a core-shell structure anti-reversal material according to claim 4, It is characterized in that The preparation of the anode slurry comprises the following steps: Anode slurry: using ionomer resin DuPont D2020 (solid content 20%), Pt / C catalyst with a platinum content of 50%, and porous carbon-wrapped iridium oxide nanoparticles prepared in the above steps, the solvent system is a solvent mixed with water and isopropanol in a ratio of 1:4; adjusting the solid content in the slurry to 2%, and the mass ratio of the dry weight of the ionomer resin to the carbon carrier of the Pt / C catalyst (IC ratio) to 0.8; using a high-speed stirrer to stir the mixed slurry, the stirring speed is set to 10000rpm, and it lasts for 30 minutes to ensure that the catalyst is fully dispersed, and then 300W ultrasonic dispersion is performed for 30 minutes. The temperature does not exceed 10°C during the entire slurry preparation process.

8. The method for preparing a core-shell structure anti-reversal material according to claim 7, It is characterized in that In the preparation of the anode slurry, the mass ratio of Pt to Ir in the catalyst slurry is controlled within a range of 30:1 to 5:

1.

9. The method for preparing a core-shell structure anti-reversal material according to claim 7, It is characterized in that In S4, the membrane electrode manufacturing specifically includes the following steps: The prepared slurry was ultrasonically sprayed, and the nozzle movement speed and discharge speed were adjusted to control the anode platinum loading to 0.1 mg / cm 2 , the cathode platinum loading is 0.35 mg / cm 2 .

10. The method for preparing a core-shell structure anti-reversal material according to claim 9, It is characterized in that In S4, during the ultrasonic spraying process, the temperature of the proton membrane carrier is 85°C; after the anode and cathode slurry spraying is completed, a 220 μm gas diffusion layer is attached to both sides of the above catalyst membrane, loaded into a mold of a hot press, and hot-pressed at 140°C and 3 MPa pressure for 2 minutes to obtain a fuel cell membrane electrode.