Slow-varying PN junction of SiC power device and generation method thereof

By adjusting the doping concentration and size of the ion implantation window in SiC power devices, a multi-layered transverse slow-changing PN junction is generated, which solves the complexity and high cost of electric field concentration caused by mutation PN junction and the existing slow-changing PN junction generation method. The problem of this achieves the matching of design and actual results and the reduction of production costs.

CN119230392APending Publication Date: 2024-12-31XPT EDS (HEFEI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310797931.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-29
Publication Date
2024-12-31

AI Technical Summary

Technical Problem

The mutation of PN junctions in existing SiC power devices leads to concentrated electric fields, the existing slow-changing PN junction generation method is complex and costly, and the photolithographic hierarchical alignment offset causes the design expectations to be inconsistent with the actual results.

Method used

By creating a mask layer on the SiC epitaxial layer, defining and adjusting the ion implantation window, performing multiple doping concentration ion implantation to form a multi-layered transverse slow-changing PN junction, avoiding multiple photolithography processes and photolithography alignments, and simplifying Process flow and reduce costs.

Benefits of technology

It realizes the generation of transversely slow-changing PN junctions without multiple lithography processes, reducing design errors and production costs, and improving device reliability and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119230392A_ABST
    Figure CN119230392A_ABST
Patent Text Reader

Abstract

The invention discloses a slowly-changing PN junction of a SiC power device and a generation method of the slowly-changing PN junction. The method comprises the steps that a mask layer is manufactured on a SiC epitaxial layer; defining an ion implantation region based on the mask layer, forming a first implantation window, and performing first doping concentration ion implantation based on the first implantation window to form a first implantation region; and reducing the first injection window by a predetermined size to form a second injection window, and performing ion injection of a second doping concentration based on the second injection window to form a second injection region, the second doping concentration being higher than the first doping concentration. According to the method, by adjusting the size of the injection window and correspondingly injecting different doping concentrations, photoetching alignment does not need to be carried out for multiple photoetching processes, so that no error exists between design expectation and an actual result, and the process complexity and the manufacturing cost are relatively low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a gradual-change PN junction of a SiC power device and a method for generating the same. Background Art

[0002] Modern power electronic devices are developing towards high power density and high efficiency. SiC power devices have developed rapidly in the field of efficient power conversion in recent years due to their excellent device characteristics such as high voltage, high frequency, high temperature and high power density. In the manufacturing process of SiC power devices, abrupt PN junctions or slow-changing PN junctions can be used for areas with concentrated electric fields such as terminals. However, abrupt PN junctions increase electric field concentration, so there is a reliability risk. For slow-changing PN junctions, the existing slow-changing PN junction generation method is usually: by using multiple photolithography plates for multiple photolithography processes, multiple etching processes and multiple ion implantation processes, a lateral slow-changing PN junction is formed (the direction of the ion implantation concentration is perpendicular to the ion implantation direction) to avoid electric field concentration. However, the complexity and production cost of this process are high, and in manufacturing, multiple photolithography processes define different implantation areas respectively, and there is a risk of alignment offset between photolithography layers, resulting in errors between design expectations and actual results. Summary of the invention

[0003] The present application provides a method for generating a gradual PN junction of a SiC power device and a gradual PN junction of a SiC power device generated by the method, so as to solve the problems of electric field concentration caused by existing abrupt PN junctions, high complexity and production cost of existing gradual PN junction manufacturing processes, and errors between design expectations and actual results caused by alignment offsets between photolithography layers.

[0004] According to one aspect of the present invention, a method for generating a gradual PN junction of a SiC power device is provided, the method comprising:

[0005] forming a mask layer on the SiC epitaxial layer;

[0006] Defining an ion implantation region based on the mask layer to form a first implantation window, and performing ion implantation of a first doping concentration based on the first implantation window to form a first implantation region;

[0007] The first injection window is reduced to a predetermined size to form a second injection window, and ions of a second doping concentration are implanted based on the second injection window to form a second injection region, wherein the second doping concentration is higher than the first doping concentration.

[0008] In some embodiments, the further step includes: expanding the second injection window by a predetermined size to form a third injection window, and performing ion implantation at a third concentration based on the third injection window to form a third injection region, wherein the third concentration is lower than the first doping concentration.

[0009] In some embodiments, reducing the first injection window to a predetermined size to form a second injection window includes: performing physical or chemical treatment on the peripheral area of ​​the remaining portion of the mask layer except the first injection window to reduce the first injection window to a predetermined size to form a second injection window.

[0010] In some embodiments, expanding the second injection window by a predetermined size to form a third injection window includes: removing the remaining portion of the mask layer except the first injection window, which has been physically or chemically treated, so that the second injection window is expanded by a predetermined size to form a third injection window.

[0011] In some embodiments, chemically treating the peripheral region of the remaining portion of the mask layer except the first injection window includes: performing oxidation treatment on the peripheral region of the remaining portion of the mask layer except the first injection window.

[0012] In some embodiments, the mask layer is polysilicon, and the peripheral region of the remaining portion of the mask layer except the first injection window is oxidized to generate silicon dioxide of a predetermined thickness.

[0013] In some embodiments, before forming a mask layer on the SiC epitaxial layer, the method further comprises: depositing an ion implantation protection layer on the surface of the SiC epitaxial layer;

[0014] The step of manufacturing a mask layer above the SiC epitaxial layer comprises: depositing the mask layer on the surface of the ion implantation protection layer.

[0015] In some embodiments, the method further includes: removing the ion implantation protection layer and the mask layer to obtain a laterally graded PN junction.

[0016] In some embodiments, defining the ion implantation area based on the mask layer to form a first implantation window includes: applying a photoresist on the surface of the mask layer, and patterning the photoresist using a photolithography process to form a patterned photoresist; and based on the patterned photoresist, using an etching process to remove a portion of the mask layer corresponding to the ion implantation area to form a first implantation window.

[0017] In some embodiments, the first injection region, the second injection region, and the third injection region are located at a main junction and / or a field limiting ring in a terminal region of the SiC power device. According to another aspect of the present invention, a graded PN junction of a SiC power device is provided, and the graded PN junction of the SiC power device is generated by the method for generating a graded PN junction of a SiC power device as described above.

[0018] Compared with the prior art, this application has the following advantages:

[0019] The method for generating a gradual PN junction of a SiC power device provided in an embodiment of the present application includes: making a mask layer above a SiC epitaxial layer; defining an ion implantation region based on the mask layer to form a first implantation window, and performing a first doping concentration ion implantation based on the first implantation window to form a first implantation region; reducing the first implantation window by a predetermined size to form a second implantation window, and performing a second doping concentration ion implantation based on the second implantation window to form a second implantation region, wherein the second doping concentration is higher than the first doping concentration. After performing a first doping concentration ion implantation based on the first implantation window to form a first implantation region, the method reduces the first implantation window by a predetermined size to form a second implantation window, and performs a second doping concentration ion implantation based on the second implantation window, wherein the second doping concentration is higher than the first doping concentration. The method adjusts the size of the implantation window and correspondingly implants different doping concentrations. The process realizes self-alignment of different ion implantation links in a simple manner, so that multiple photolithography processes are not required in the PN junction generation process, and photolithography alignment is not required for multiple photolithography processes, so that there is no error between the design expectation and the actual result, and the process complexity and production cost are low.

[0020] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the following specifically cites the preferred embodiments and describes them in detail with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic flow chart of a method for generating a slowly varying PN junction of a SiC power device provided in an embodiment of the present application;

[0022] Figure 2-Figure 9 A schematic diagram of a process for manufacturing a gradual-change PN junction of a SiC power device provided in this embodiment;

[0023]

Explanation of symbols

[0024] Mask layer 1, ion implantation protection layer 2, first implantation window 3, first implantation region 4, second implantation window 5, second implantation region 6, third implantation window 7, second implantation region 8, main junction 9, field limiting ring 10 DETAILED DESCRIPTION

[0025] Many specific details are described in the following description to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present application, so the present application is not limited by the specific implementation disclosed below.

[0026] Compared with traditional silicon (Si) materials, silicon carbide (SiC) has the advantages of wide bandgap, high critical breakdown electric field, large saturation drift velocity and high thermal conductivity. It is an ideal material for preparing high-voltage and high-power devices. It is widely used in high-efficiency, high-power and high-temperature power electronics technology and has become a research hotspot in current power semiconductor technology. In the manufacturing process of SiC power devices, abrupt PN junctions or slow-changing PN junctions can be used for areas with concentrated electric fields such as terminals. In the field of semiconductor technology, different doping processes are used to make P-type semiconductors and N-type semiconductors on the same semiconductor substrate through diffusion. The space charge region formed near the interface of the two semiconductors is called a PN junction. The PN junction has unidirectional conductivity, which is a characteristic used by many devices in electronic technology, such as semiconductor diodes and bipolar transistors. A graded pn junction refers to a PN junction in which the doping concentration gradually changes from the p region to the n region. For example, a PN junction manufactured using a solid-state diffusion process, that is, the p region and the n region are non-uniformly doped. Under thermal equilibrium, the electric field distribution of the graded pn junction is nonlinear.

[0027] In high-voltage applications, a sudden PN junction is prone to electric field concentration at the corner of the PN junction, which reduces the breakdown voltage of the device and poses a reliability risk. For a gradual PN junction, the existing method for generating a gradual PN junction is generally to use multiple photolithography processes (defining the injection area by photolithography), multiple etching processes, and multiple ion implantation processes (for example, a low concentration is implanted for the first time and a high concentration is implanted for the second time) using multiple photomasks to form a lateral gradual PN junction (a lateral gradual PN junction is a PN junction in which the doped ion implantation concentration varies horizontally) to avoid electric field concentration. However, the process is complex and has a high production cost. In addition, during manufacturing, multiple photolithography processes are used to define different implantation areas, and there is a risk of misalignment between different photolithography levels, resulting in an unstable distance between the low-doping boundary and the high-doping boundary in the gradual PN junction, which in turn leads to an error between the design expectations and actual results of the gradual PN junction.

[0028] In view of the above problems, in order to avoid the electric field concentration caused by the sudden PN junction, the complexity and high production cost of the existing slow-changing PN junction manufacturing process, and the error between the design expectation and the actual result caused by the offset between the photolithography levels, and in the silicon process device, the slow-changing PN junction is realized by a thermal process, but since the impurity diffusion coefficient in the SiC substrate is extremely low, it is difficult for the injected impurities to diffuse laterally, and therefore a lateral slow-changing PN junction cannot be formed in the SiC substrate by a thermal process. Based on this, the embodiment of the present application is directed to a lateral slow-changing PN junction, and provides a method for generating a slow-changing PN junction of a SiC power device and a slow-changing PN junction of a SiC power device generated by the method. Please refer to Figure 1 , Figure 2-Figure 9 To understand this embodiment, Figure 1 A schematic diagram of a flow chart of a method for generating a slowly varying PN junction of a SiC power device provided in this embodiment; Figure 2-Figure 9 A schematic diagram of a process for manufacturing a gradual-change PN junction of a SiC power device provided in this embodiment.

[0029] like Figure 1-Figure 9 As shown, the method for generating a gradual PN junction of a SiC power device provided in this embodiment includes the following steps:

[0030] S1: a mask layer 1 is formed on the SiC epitaxial layer. Specifically, after a lightly doped SiC epitaxial layer is grown on the upper surface of a heavily doped SiC substrate, an ion implantation protection layer 2 is deposited on the surface of the SiC epitaxial layer, and a mask layer 1 is deposited on the surface of the ion implantation protection layer 2. In this embodiment, the ion implantation protection layer 2 may be silicon nitride, and the mask layer 1 may be polycrystalline silicon (e.g. Figure 2 shown).

[0031] S2: Based on the mask layer 1, define the ion implantation area to form a first implantation window 3, and perform ion implantation of a first doping concentration based on the first implantation window 3 to form a first implantation region 4; in this embodiment, the first implantation window 3 (such as Figure 3 Specifically, a photoresist may be coated on the surface of the mask layer, and the photoresist may be patterned by a photolithography process to form a patterned photoresist. Then, based on the patterned photoresist, an etching process may be used to remove a portion of the mask layer corresponding to the ion implantation region to form a first implantation window. Figure 4 As shown, the first doping concentration ion implantation based on the first implantation window 3 may specifically refer to: Al ion implantation with a medium doping concentration is performed through the first implantation window, the implantation energy may be 380 KeV, and the implantation dose may be 2.5E13 atoms per square centimeter.

[0032] S3: Reduce the first injection window to a predetermined size to form a second injection window 5 (eg Figure 5As shown), and based on the second injection window 5, a second doping concentration ion implantation is performed to form a second injection region 6 (as shown Figure 6 As shown), wherein the second doping concentration is higher than the first doping concentration, high doping concentration Al ion implantation can be performed through the second implantation window 5, the implantation energy can be 525Kev, and the implantation dose can be 5.5E13 atoms per square centimeter.

[0033] The above-mentioned reduction of the first injection window to a predetermined size may refer to: performing physical or chemical treatment on the peripheral area of ​​the remaining part of the mask layer except the first injection window, so that the peripheral area of ​​the remaining part of the mask layer can be uniformly expanded. The above-mentioned physical treatment method may be to uniformly fill the peripheral area of ​​the remaining part of the mask layer with a filler, or to expand the volume of the peripheral area by deposition, or to expand the peripheral area of ​​the remaining part of the mask layer by other volume expansion methods, for example, uniformly depositing or filling other solid substances in the peripheral area of ​​the remaining part of the mask layer, so that the width or volume of the remaining part of the mask layer can be expanded to a preset size.

[0034] The above-mentioned chemical treatment refers to causing a chemical reaction in the peripheral area of ​​the remaining part of the above-mentioned mask layer to expand the volume or width of the remaining part of the mask layer to a preset size. For example, the peripheral area of ​​the remaining part of the mask layer except the first injection window is oxidized. In the present embodiment, the mask layer can be polycrystalline silicon, which is wet-oxidized to generate silicon dioxide. To grow silicon dioxide with a width of 1 micron, 0.44 microns of polycrystalline silicon are required. Based on this conversion relationship, the size of the first injection window to be reduced or the size of the second injection window can be preset, as well as the size of the remaining part of the mask layer except the first injection window that does not require oxidation treatment, and the degree of oxidation of the polycrystalline silicon is controlled based on these preset sizes to obtain a second injection window that meets the size requirements.

[0035] After the first doping concentration ion implantation is performed based on the first implantation window to form a first implantation area, the peripheral area of ​​the remaining portion of the mask layer is physically or chemically treated to reduce the first implantation window to a predetermined size to form a second implantation window, and the second doping concentration ion implantation is performed based on the second implantation window, wherein the second doping concentration is higher than the first doping concentration. The method adjusts the size of the implantation window by physically or chemically treating the peripheral area of ​​the remaining portion of the mask layer, and injects different doping concentrations accordingly. The process achieves self-alignment of different ion implantation processes in a simple manner, so that multiple photolithography processes are not required in the process of generating a lateral gradual PN junction, and photolithography alignment is not required for multiple photolithography processes, so that there is no error between the design expectation and the actual result, and the process complexity and production cost are low.

[0036] It should be noted that in order to make the doping concentration of the generated gradual PN junction present multi-level characteristics to better avoid electric field concentration, the method provided in this embodiment may also include the following steps:

[0037] S4: Enlarging the second injection window by a predetermined size to form a third injection window 7, and performing ion implantation of a third concentration based on the third injection window 7 to form a third injection region 8, wherein the third concentration is lower than the first doping concentration. Specifically, the remaining portion of the mask layer except the first injection window and the portion that has been physically or chemically treated may be removed to expand the second injection window by a predetermined size, for example, by using a hydrofluoric acid etching method in a wet etching back process to remove silicon dioxide, leaving only unoxidized polysilicon, the width of the removed silicon dioxide corresponding to the size of the second injection window being enlarged, and the unoxidized polysilicon forming the third injection window (such as Figure 7 Then, a low-doping concentration Al ion implantation is performed through the third implantation window. The implantation energy may be 180 KeV, and the implantation dose may be 5E12 atoms per square centimeter (as shown in FIG. Figure 8 shown).

[0038] S5: Remove the ion implantation protection layer 2 and the mask layer 1 (the remaining part) to obtain a lateral graded PN junction (such as Fig. 9 As shown), for example, a CMP process or a dry etching back process is used to remove silicon nitride on the surface of the SiC epitaxial layer and polysilicon that has not been oxidized. CMP (Chemical Mechanical Polishing) uses a process that combines mechanical friction and chemical corrosion to flatten the surface of the semiconductor material. Compared with mechanical polishing, the CMP process can make the surface of the semiconductor material flatter and the processing method is simpler.

[0039] In this embodiment, since the terminal region of the SiC power device is a region of concentrated electric field, the first injection region, the second injection region and the third injection region are located in the main junction of the terminal region of the SiC power device, or in the field limiting ring of the terminal of the SiC power device, or in the main junction 9 and the field limiting ring 10 of the terminal region of the SiC power device (such as Figure 3-Figure 9 As shown, a lateral graded PN junction is formed in the main junction 9 and each field limiting ring 10 at the terminal of the SiC power device by the above-mentioned method).

[0040] Through the above method, the ion implantation area can be made into a second implantation area with high doping concentration ions, a first implantation area with medium doping concentration ions and a third implantation area with low doping concentration ions from the inside to the outside, that is, the doping concentration of the formed gradual PN junction gradually decreases from its central area to the peripheral area (in the lateral direction and the longitudinal direction), and has a multi-level nature, so that the charge concentration changes in a gradient and gradually decreases evenly, which can effectively alleviate the electric field concentration phenomenon. Furthermore, in the above method, only one photolithography process is required to generate the first injection window. After that, the size of the injection window is adjusted by physically or chemically treating the peripheral area of ​​the remaining part of the mask layer except the first injection window (for example, oxidizing polysilicon to silicon dioxide) and removing the physically or chemically treated part of the mask layer. The injection area is defined in a self-aligned manner (that is, during two or more ion implantations, the relative position of the implantation area remains unchanged and no offset occurs). Based on this, multiple ion implantations are performed to laterally generate a multi-layer ion implantation structure. This process does not require photolithography alignment for multiple photolithography processes, and only one photolithography process is required to laterally generate a multi-layer ion implantation structure. The requirement for the maximum line width of the photolithography machine can be reduced in a self-aligned manner (that is, since the ion implantation process only requires one photolithography process, the subsequent self-alignment method replaces multiple photolithography processes, and a line width design that exceeds the production line capacity of the photolithography machine can be achieved. For example, Figure 3 It is shown in the figure that the limit line width of the lithography machine is 0.8um, making Figure 4 The distance between the main junction and the field limiting ring formed after ion implantation is 0.8um. Figure 7 and Figure 8 After that, the distance between the main junction and the field limiting ring can be reduced to 0.4um (the closer the distance between the main junction and the first field limiting ring is, the better the electric field distribution is). This distance has exceeded the limit line width of the lithography machine, which is equivalent to using a lithography machine with a limit line width of 0.8 microns to achieve a 0.4 micron structural effect. Therefore, using this method, a line width design that exceeds the production line capacity of the lithography machine can be achieved, thereby reducing the requirement for the limit line width of the lithography machine), and simultaneously realizing the alignment requirements of each ion implantation link, so that there is no error between the design expectation and the actual result for the slow-varying PN junction, the process complexity is reduced, and the production cost is reduced.

[0041] Another embodiment of the present application further provides a gradually varying PN junction of a SiC power device, wherein the gradually varying PN junction of the SiC power device is a lateral gradually varying PN junction generated by the gradually varying PN junction generating method of the SiC power device provided by the above-mentioned embodiment. For the specific contents of the lateral gradually varying PN junction, please refer to the relevant description of the above-mentioned embodiment, which will not be repeated here.

[0042] It should be noted that although the present application is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present application. Any technical personnel in this field may make possible changes and modifications without departing from the spirit and scope of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A method for generating a slow-changing PN junction of a SiC power device, characterized in that: The method comprises: forming a mask layer on the SiC epitaxial layer; Defining an ion implantation region based on the mask layer to form a first implantation window, and performing ion implantation of a first doping concentration based on the first implantation window to form a first implantation region; The first injection window is reduced to a predetermined size to form a second injection window, and ions of a second doping concentration are implanted based on the second injection window to form a second injection region, wherein the second doping concentration is higher than the first doping concentration.

2. The method according to claim 1, characterized in that The method further comprises: The second implantation window is enlarged to a predetermined size to form a third implantation window, and ions are implanted at a third concentration based on the third implantation window to form a third implantation region, wherein the third concentration is lower than the first doping concentration.

3. The method according to claim 2, characterized in that The first injection window is reduced to a predetermined size to form a second injection window, comprising: The peripheral area of ​​the remaining portion of the mask layer except the first injection window is physically treated or chemically treated to reduce the first injection window to a predetermined size, thereby forming a second injection window.

4. The method according to claim 3, characterized in that The step of expanding the second injection window by a predetermined size to form a third injection window includes: removing the physically or chemically treated portion of the remaining portion of the mask layer except the first injection window, so as to expand the second injection window by a predetermined size to form a third injection window.

5. The method according to claim 3, characterized in that: The chemical treatment of the peripheral area of ​​the remaining portion of the mask layer except the first injection window comprises: An oxidation process is performed on the peripheral area of ​​the remaining portion of the mask layer except the first implantation window.

6. The method according to claim 5, characterized in that The mask layer is polysilicon, and after the peripheral area of ​​the remaining part of the mask layer except the first injection window is oxidized, silicon dioxide with a predetermined thickness is generated.

7. The method according to claim 1 or 2, characterized in that: Before forming a mask layer on the SiC epitaxial layer, the method further comprises: depositing an ion implantation protection layer on the surface of the SiC epitaxial layer; The step of manufacturing a mask layer above the SiC epitaxial layer comprises: depositing the mask layer on the surface of the ion implantation protection layer.

8. The method according to claim 7, characterized in that The method further comprises: removing the ion implantation protection layer and the mask layer to obtain a laterally graded PN junction.

9. The method according to claim 1, characterized in that: The step of defining an ion implantation region based on the mask layer to form a first implantation window comprises: Applying photoresist on the surface of the mask layer, and patterning the photoresist using a photolithography process to form a patterned photoresist; According to the patterned photoresist, an etching process is adopted to remove a portion of the mask layer corresponding to the ion implantation area to form a first implantation window.

10. The method according to claim 2, characterized in that The first implantation region, the second implantation region and the third implantation region are located at a main junction and / or a field limiting ring in a terminal region of the SiC power device.

11. A gradual change PN junction of a SiC power device, characterized in that: The gradual change PN junction of a SiC power device is generated by the gradual change PN junction generation method of a SiC power device according to any one of claims 1 to 10.