Paint proportioning process for wiredrawing rose gold nano coating for decorative plate product

By adding silicon powder to the brushed rose gold nanocoated paint and heating and stirring, the problem of nanocoated paint being prone to scratches on the surface of the decorative board is solved, and the wear resistance and protection ability of the paint is improved.

CN119410269AInactive Publication Date: 2025-02-11ZHAOQING HONGWANG METAL IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411322381.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2025-02-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When used on the surface of decorative panels, existing nano-coated paints are susceptible to scratches caused by external forces, reducing their protection capabilities.

Method used

The paint with a complete silicon molecular structure is formed by adding a certain amount of silicon powder to the ratio of the brushed rose gold nanocoated paint and blending it into the solution during heating and stirring.

Benefits of technology

It improves the wear resistance of paint, ensures the normal color performance and the purity of paint, and enhances its protection ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119410269A_ABST
    Figure CN119410269A_ABST
Patent Text Reader

Abstract

The invention discloses a paint proportioning process for a wiredrawing rose gold nano coating for a decorative plate product, which comprises the following steps: step 1, selecting a proper amount of nano wear-resistant paint, a silane coupling agent, rosin resin, amber resin, benzoin resin, calcium plumbate, silica gel, iron powder, mica powder, citric acid, silicon powder, water and a thinner, and putting the selected materials into a stirrer for stirring, the stirring speed is 300-400 revolutions per minute, the stirring time is 10-20 minutes, and the stirring temperature is controlled to be 45-65 DEG C; the preparation method has the beneficial effects that a certain amount of silicon powder is added in the proportioning process, the silicon powder can be fused into a solution in the subsequent heating and stirring process, the silicon molecular structure is very complete, and no grain boundary or impurity exists, so that the normal color of the paint can be ensured, the purity of the paint can be ensured, and the wear resistance of the paint is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of brushed rose gold nano coating paint ratio, and the invention relates to a brushed rose gold nano coating paint ratio process for a decorative plate product. Background Art

[0002] Nano paint is a special paint prepared using nano technology and has many excellent performance characteristics. Rose gold nano coating paint generally refers to a special paint with metallic color and nano-level particles. When existing nano coating paint is used on the surface of decorative panels, the nano coating paint is in direct contact with the outside world and is easily scratched by external forces, reducing its protective ability. Summary of the invention

[0003] The purpose of the present invention is to provide a brushed rose gold nano-coating paint mixing process for decorative panel products in order to solve the above-mentioned problems.

[0004] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0005] A brushed rose gold nano-coating paint mixing process for decorative board products, comprising the following steps:

[0006] Step 1: Select appropriate amounts of nano wear-resistant paint, silane coupling agent, rosin resin, amber resin, benzoin, calcium lead acid, silica gel, iron powder, mica powder, citric acid, silicon powder, water and thinner, and put the selected materials into a blender for stirring at a speed of 300-400 rpm for 10-20 minutes, and the stirring temperature is controlled at 45°C-65°C;

[0007] Step 2: Add appropriate amounts of stabilizer, thickener and defoamer to the solution formed by stirring in step 1, and stir, and finally add appropriate amounts of deionized water, ethanol and mica powder and stir together to obtain a mixed solution;

[0008] Step 3: The mixed solution obtained in step 2 is fully mixed by a mixer, the speed is controlled at 250-350 rpm, and then the temperature is raised to 50°C-55°C, and magnetically stirred for 30-40 minutes, and then the mixture is filtered and allowed to stand for 20-24 hours, and the supernatant is removed to obtain the rose gold nano-coating paint.

[0009] Furthermore, in the step 1, the rosin resin, amber resin, benzoic acid resin, calcium plumbic acid, iron powder and mica powder are poured into a grinder for grinding for 20-30 minutes until the particle size reaches 3000-4000 meshes, thereby obtaining a mixed powder, which needs to be filtered after grinding.

[0010] Furthermore, in the step 1, the batching needs to be completed twice, and after the single batching is completed, the remaining components need to be supplemented and then dispersed and mixed.

[0011] Furthermore, the stirring time after adding the stabilizer, thickener and defoamer in step 2 is controlled at 20-25 minutes, the stirring temperature is raised to 70° C.-90° C., and the stirring rate is controlled at 200-300 rpm.

[0012] Furthermore, in step 2, the stirring time of adding deionized water, ethanol and mica powder is controlled to be 30-45 minutes, the stirring temperature is increased to 70° C.-90° C., and the stirring rate is controlled to be 250-350 rpm.

[0013] Furthermore, a sand mill, a ball mill and a three-roll mill can be used in the grinding process according to the use requirements.

[0014] Furthermore, after grinding, the ground material is filtered through a plate and frame filter, a centrifugal filter or a bag filter.

[0015] Furthermore, in step 1, when mixing and stirring the raw materials, a lifting stirring method is adopted in the stirring equipment.

[0016] The beneficial effects of the present invention are:

[0017] The present invention adds a certain amount of silicon powder during the proportioning process, and the silicon powder can be integrated into the solution during the subsequent heating and stirring process. The silicon molecular structure is very complete, without crystal boundaries and impurities, which can ensure the normal color of the paint, the purity of the paint, and increase the wear resistance of the paint. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention provides a flow chart of a paint proportioning process for a brushed rose gold nano-coating used for a decorative panel product. DETAILED DESCRIPTION

[0019] A brushed rose gold nano-coating paint mixing process for decorative board products, comprising the following steps:

[0020] Step 1: Select appropriate amounts of nano wear-resistant paint, silane coupling agent, rosin resin, amber resin, benzoin, calcium lead acid, silica gel, iron powder, mica powder, citric acid, silicon powder, water and thinner, and put the selected materials into a blender for stirring at a speed of 300-400 rpm for 10-20 minutes, and the stirring temperature is controlled at 45°C-65°C;

[0021] Step 2: Add appropriate amounts of stabilizer, thickener and defoamer to the solution formed by stirring in step 1, and stir, and finally add appropriate amounts of deionized water, ethanol and mica powder and stir together to obtain a mixed solution;

[0022] Step 3: The mixed solution obtained in step 2 is fully mixed by a mixer, the speed is controlled at 250-350 rpm, and then the temperature is raised to 50°C-55°C, and magnetically stirred for 30-40 minutes, and then the mixture is filtered and allowed to stand for 20-24 hours, and the supernatant is removed to obtain the rose gold nano-coating paint.

[0023] In this embodiment, in the step 1, rosin resin, amber resin, benzoic acid resin, calcium plumbic acid, iron powder and mica powder are poured into a grinder for grinding for 20-30 minutes to reach a particle size of 3000-4000 mesh to obtain a mixed powder, which needs to be filtered after grinding.

[0024] In this embodiment, when batching in step 1, the batching needs to be completed twice, and after the single batching is completed, the remaining components need to be supplemented and then dispersed and mixed.

[0025] In this embodiment, the stirring time after adding the stabilizer, thickener and defoamer in step 2 is controlled at 20-25 minutes, the stirring temperature is raised to 70° C.-90° C., and the stirring rate is controlled at 200-300 rpm.

[0026] In this embodiment, the stirring time of adding deionized water, ethanol and mica powder in step 2 is controlled at 30-45 minutes, the stirring temperature is increased to 70° C.-90° C., and the stirring rate is controlled at 250-350 rpm.

[0027] In this embodiment, a sand mill, a ball mill and a three-roll mill can be used in the grinding process according to usage requirements.

[0028] In this embodiment, after grinding, the ground material is filtered through a plate and frame filter, a centrifugal filter or a bag filter.

[0029] In this embodiment, in step 1, when mixing and stirring the raw materials, a lifting stirring method is adopted in the stirring equipment.

[0030] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A brushed rose gold nano-coating paint mixing process for decorative board products, characterized by: It includes the following steps: Step 1: Select appropriate amounts of nano wear-resistant paint, silane coupling agent, rosin resin, amber resin, benzoin, calcium lead acid, silica gel, iron powder, mica powder, citric acid, silicon powder, water and thinner, and put the selected materials into a blender for stirring at a speed of 300-400 rpm for 10-20 minutes, and the stirring temperature is controlled at 45°C-65°C; Step 2: Add appropriate amounts of stabilizer, thickener and defoamer to the solution formed by stirring in step 1, and stir, and finally add appropriate amounts of deionized water, ethanol and mica powder and stir together to obtain a mixed solution; Step 3: The mixed solution obtained in step 2 is fully mixed by a mixer, the speed is controlled at 250-350 rpm, and then the temperature is raised to 50°C-55°C, and magnetically stirred for 30-40 minutes, and then the mixture is filtered and allowed to stand for 20-24 hours, and the supernatant is removed to obtain the rose gold nano-coating paint.

2. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 1, characterized in that: In the step 1, rosin resin, amber resin, benzoic acid resin, calcium plumbic acid, iron powder and mica powder are poured into a grinder for grinding for 20-30 minutes until the particle size reaches 3000-4000 meshes, thereby obtaining a mixed powder, which needs to be filtered after grinding.

3. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 1 is characterized by: When batching in step 1, the batching needs to be completed twice. After the single batching is completed, the remaining components need to be supplemented and then dispersed and mixed.

4. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 1, characterized in that: The stirring time after adding the stabilizer, thickener and defoamer in step 2 is controlled at 20-25 minutes, the stirring temperature is raised to 70° C.-90° C., and the stirring rate is controlled at 200-300 rpm.

5. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 1 is characterized by: The stirring time of adding deionized water, ethanol and mica powder in step 2 is controlled to be 30-45 minutes, the stirring temperature is increased to 70° C.-90° C., and the stirring rate is controlled to be 250-350 rpm.

6. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 2, characterized in that: During the grinding process, a sand mill, a ball mill and a three-roll mill can be used according to the requirements.

7. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 2 is characterized by: After grinding, the ground material is filtered through a plate and frame filter, a centrifugal filter or a bag filter.

8. The paint mixing process for drawing rose gold nano coating for decorative board products according to claim 1 is characterized by: In the step 1, when mixing and stirring the raw materials, a lifting stirring method is adopted in the stirring equipment.