A 5A molecular sieve for pressure swing adsorption and its preparation method
By coating the surface of NaA molecular sieve raw powder with melamine cyanurate and combining it with magnesium hydroxide whiskers, calcium peroxide powder and calcium carbonate whiskers, the problems of low adsorption capacity and poor mechanical strength of 5A molecular sieves were solved, and 5A molecular sieves with high adsorption capacity and long service life were prepared.
Patent Information
- Application Number
- CN202611627453.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing 5A molecular sieves for pressure swing adsorption have problems such as low adsorption capacity, poor mechanical strength, and short service life.
The surface of NaA molecular sieve powder is coated with melamine cyanurate, combined with magnesium hydroxide whiskers and calcium peroxide powder as pore-forming agents, and through-hole channels are formed by calcination. Calcium carbonate whiskers are used to enhance mechanical properties, and finally calcium exchange and drying activation are carried out.
A 5A molecular sieve with high adsorption capacity, strong crushing resistance, and low wear rate was prepared, with a nitrogen adsorption capacity of 21.45~24.83 mL/g, which significantly improved its service life.
Smart Images

Figure CN123102300A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a 5A molecular sieve for pressure swing adsorption and its preparation method, belonging to the field of adsorption separation technology. Background Technology
[0002] Pressure swing adsorption (PSA), as a chemical engineering unit technology, is now widely used for the separation and purification of mixed gases. With the development of PSA technology and the scaling up of equipment, such as those with a processing capacity of 200,000 Nm³, the application of PSA technology has become increasingly sophisticated. 3 The / hr hydrogen separation and purification device places higher demands on the adsorbent, requiring high adsorption capacity, fast adsorption and desorption rates, and high mechanical strength. 5A molecular sieves, used as adsorbents for pressure swing adsorption (PSA) in oxygen production, hydrogen and carbon monoxide purification, and dewaxing in petroleum refineries, are traditionally produced by mixing 4A molecular sieve powder with kaolin, granulating, drying, calcining, CaCl2 exchange, and drying activation to obtain 5A molecular sieves. Currently, 5A molecular sieves produced on a large scale using this traditional method still suffer from prominent problems such as low adsorption capacity, poor mechanical strength, and short service life.
[0003] Chinese patent CN114433014A discloses a method for preparing a 5A molecular sieve adsorbent. The method involves mixing 4A molecular sieve powder, clay, soda ash, additives, and water in a specific ratio to obtain a wet material clump, which is then shaped into strip-shaped particles. These particles are then rolled to obtain spherical particles. The spherical particles are dried and calcined. The calcined material undergoes a crystallization reaction, causing the binder to transform from a solid to a crystal. The resulting product undergoes ion exchange in a calcium solution, followed by drying and calcination to obtain the 5A molecular sieve adsorbent. The nitrogen adsorption capacity of the 5A molecular sieve adsorbent obtained by this patent is relatively low, with a maximum value of only 15.3 mL / g.
[0004] Chinese patent CN114682237A discloses a method for preparing a high-efficiency 5A molecular sieve adsorbent. First, the raw 5A molecular sieve powder is carboxylated and modified to obtain a modified 5A molecular sieve. The modified 5A molecular sieve, binder, sodium hydroxide, and binding aid are mixed and then molded. The resulting intermediate is dried and calcined to obtain the 5A molecular sieve adsorbent. The adsorbent obtained by this patent has a very low maximum adsorption capacity for nitrogen, only 12.1 mL / g. Furthermore, it does not disclose any measures to enhance the mechanical properties of the molecular sieve adsorbent; its strength is not improved, and its service life is not very long.
[0005] As can be seen from the above, the 5A molecular sieves used in pressure swing adsorption still have significant problems such as low adsorption capacity, poor mechanical strength, and limited service life. Therefore, it is urgent to develop 5A molecular sieves for pressure swing adsorption with high adsorption capacity, high strength, and long service life. Summary of the Invention
[0006] To address the shortcomings of the existing technology, this invention provides a 5A molecular sieve for pressure swing adsorption and its preparation method, achieving the following objective: to prepare a 5A molecular sieve for pressure swing adsorption with high adsorption capacity, high strength, and long service life.
[0007] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A 5A molecular sieve for pressure swing adsorption and its preparation method, wherein the 5A molecular sieve for pressure swing adsorption has a crushing force of 61.4~67.9N, an abrasion rate of 0.08~0.16%, and a nitrogen adsorption capacity of 21.45~24.83mL / g; The preparation method of the 5A molecular sieve for pressure swing adsorption includes five steps: coating the surface of NaA molecular sieve raw powder, mixing and molding, calcination, calcium exchange, and drying and activation. The following are further improvements to the above technical solution:
[0008] Step 1: Coating the surface of NaA molecular sieve powder NaA molecular sieve raw powder and deionized water were placed in a reaction vessel and heated to the reaction temperature while stirring. An amino-containing silane coupling agent was added at a constant temperature. After the reaction was complete, saturated melamine aqueous solution and saturated cyanuric acid aqueous solution, which were preheated to the reaction temperature and kept at a constant temperature, were added dropwise to the vessel. The dropping rate of the two saturated solutions was controlled so that melamine and cyanuric acid were added dropwise to the reaction vessel at a molar ratio of 1:1. After the addition was completed, the temperature was kept constant until the reaction was completed. Then, the mixture was filtered, washed, and dried to obtain NaA molecular sieve raw powder with melamine cyanurate coated on the surface. The particle size of the NaA molecular sieve raw powder is 2~7μm; The amino-containing silane coupling agent is at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and ureapropyltriethoxysilane. The mass ratio of the NaA molecular sieve raw powder, deionized water, amino-containing silane coupling agent, and saturated melamine aqueous solution is 40~130:400~1900:3~13:960~3800; The dropping rate of the saturated melamine aqueous solution is 120~800 g / min; The reaction temperature is 60~85℃; Under the specified stirring conditions, the stirring rate is 800~1600 rpm; After the reaction is complete, the reaction time is 2 to 4.5 hours; The temperature is maintained at a constant level until the reaction is complete, and the reaction time is 1 to 3.5 hours. The washing process involves washing with deionized water 2-3 times, with the mass of deionized water used in each wash being equal to the mass of the wet solid being washed. The drying process involves a drying temperature of 85-110℃ and a drying time of 15-24 hours.
[0009] Step 2: Mixing and Molding NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, and deionized water are added to a double planetary mixer and stirred at high speed until initially mixed. Then, calcium peroxide powder is added and stirred at high speed until mixed a second time. Then, magnesium aluminum silicate is added and stirred at high speed until mixed a third time. The resulting viscous slurry is transferred into a granulator and formed into spherical particles. The silicate is at least one of potassium silicate and sodium metasilicate; The calcium carbonate whiskers have a diameter of 0.5~3μm and a length of 8~30μm; The magnesium hydroxide whiskers have a diameter of 0.1~1μm and a length of 6~20μm; The kaolin has a particle size of 0.2~6μm; The particle size of the calcium peroxide powder is 0.1~1.3μm; The mass ratio of the NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, deionized water, calcium peroxide powder, and magnesium aluminum silicate is 50~360:2~40:3~35:5~40:10~60:260~1000:2~25:1~5; The high-speed stirring has a stirring rate of 300~550 rpm. The initial mixing is uniform, and the mixing time is 3-6 hours; The secondary mixing process takes 1 to 2 hours. The three mixing processes are carried out over a period of 0.6 to 1.5 hours. The diameter of the spherical particles is 2-7 mm.
[0010] Step 3, roasting After the spherical particles are initially dried and cured at 90~130℃ for 1~3.5 hours, they are then calcined at 500~660℃ for 3~6 hours at a rate of 3~5℃ / min, and then cooled to room temperature to obtain the calcined molecular sieve.
[0011] Step 4, Calcium Exchange The calcined molecular sieve is placed in a calcium chloride aqueous solution and exchanged at a constant temperature of 70~95℃ for 3~7 hours, and then filtered to obtain the calcium-exchanged molecular sieve. The concentration of the calcium chloride aqueous solution is 0.1~1 mol / L; The mass ratio of the calcined molecular sieve to the calcium chloride aqueous solution is 10:33~70.
[0012] Step 5: Drying and Activation The calcium-exchanged molecular sieve is dried at 85~130℃ for 15~35 hours, and then activated at 550~750℃ for 1.5~4 hours at a heating rate of 1~4℃ / min to obtain 5A molecular sieve for pressure swing adsorption.
[0013] Compared with the prior art, the present invention achieves the following beneficial effects: 1. During the sintering process of molecular sieve raw powder, the added sintering aids (or binders, which sinter the molecular sieve raw powder particles into a whole through high-temperature sintering), such as silicates and kaolin in this invention, will undergo dense sintering and over-coating with the surface of the molecular sieve raw powder particles, thus completely blocking the contact between the internal micropores of the molecular sieve raw powder particles and the outside world. Gas molecules or calcium ions in the calcium exchange process cannot enter the internal micropores of the molecular sieve raw powder particles, thus leading to the inability to carry out effective calcium exchange or gas adsorption. To solve the above problems, this invention coats the surface of NaA molecular sieve raw powder particles with melamine cyanurate. The main coating mechanism is as follows: first, the surface of NaA molecular sieve raw powder particles is modified with an amino-containing silane coupling agent. After the hydroxyl groups on the surface of the molecular sieve particles react with the amino-containing silane coupling agent, the NaA molecular sieve raw powder particles... The surface is covered with amino groups. Then, melamine and cyanuric acid react in a 1:1 molar ratio to generate melamine cyanurate. During this process, because the amino groups covering the surface of the NaA molecular sieve powder particles have strong hydrogen bonding with melamine, cyanuric acid, and melamine cyanurate, melamine cyanurate preferentially uses the NaA molecular sieve powder particles as the nucleus and undergoes a precipitation reaction. In this way, melamine cyanurate forms a relatively dense coating layer on the surface of the NaA molecular sieve powder particles through hydrogen bonding. During the subsequent calcination process, melamine cyanurate undergoes thermal decomposition, generating micropores on the surface of the NaA molecular sieve powder particles. These micropores can completely avoid the dense sintering coating effect of sintering aids on the surface of the NaA molecular sieve powder particles. At the same time, these micropores provide a large number of channels for calcium ions and gas molecules to enter the interior of the molecular sieve powder particles. 2. To create more interconnected channels within the 5A molecular sieve for pressure swing adsorption (PSA) and improve the rate of gas diffusion into the molecular sieve, this invention specifically incorporates two pore-forming agents: magnesium hydroxide whiskers and calcium peroxide powder. Magnesium hydroxide whiskers, through thermal decomposition, effectively form continuous interconnected pores, while the finer calcium peroxide particles create smaller pores. This combination offers two main advantages: first, the interconnected channels formed by the magnesium hydroxide whiskers connect the smaller pores created by the calcium peroxide, forming a continuous, interconnected pore structure within the sintered molecular sieve body; second, the smaller particle size of the pores formed by the calcium peroxide minimizes its impact on the overall mechanical properties of the 5A molecular sieve for PSA. This structure, combining through-holes and small pores, effectively affects mechanical properties. It maximizes the channels for calcium ions and gas molecules to diffuse in and out of the 5A molecular sieve used in pressure swing adsorption (PSA). This allows each molecular sieve powder particle inside the 5A molecular sieve to effectively contact calcium ions or gas molecules during calcium exchange or gas adsorption. Furthermore, the calcium oxide formed after the thermal decomposition of calcium peroxide will generate calcium hydroxide during the calcium exchange step. The calcium ions released by the calcium hydroxide dissolution can promote calcium exchange to a certain extent, thus increasing the calcium content in the final 5A molecular sieve used in PSA. The increase in calcium content will significantly improve the nitrogen adsorption capacity of the molecular sieve. 3. In this invention, calcium carbonate whiskers are used to enhance the mechanical properties of 5A molecular sieves for pressure swing adsorption. Calcium carbonate whiskers have strong surface polarity and excellent compatibility with silicates and kaolin, making them easy to mix evenly with silicates and kaolin. Moreover, during sintering, the polar functional groups on the surface of calcium carbonate whiskers easily react with silicates and kaolin to form a dense sintered body, thereby achieving a good strengthening effect. 4. The 5A molecular sieve for pressure swing adsorption prepared by this invention has a crushing force of 61.4~67.9N, an abrasion rate of 0.08~0.16%, and a nitrogen adsorption capacity of 21.45~24.83mL / g. Attached Figure Description
[0014] Figure 1 The image shows a scanning electron microscope (SEM) image of the cross-section of the 5A molecular sieve for pressure swing adsorption obtained in Example 1, magnified 3000 times. Figure 2 The image shown is a scanning electron microscope (SEM) image of the cross-section of the 5A molecular sieve for pressure swing adsorption obtained in Example 1, magnified 6000 times. Detailed Implementation
[0015] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0016] Example 1: A method for preparing 5A molecular sieves for pressure swing adsorption Step 1: Coating the surface of NaA molecular sieve powder NaA molecular sieve raw powder and deionized water were placed in a reaction vessel and heated to the reaction temperature while stirring. An amino-containing silane coupling agent was added at a constant temperature. After the reaction was complete, saturated melamine aqueous solution and saturated cyanuric acid aqueous solution, which were preheated to the reaction temperature and kept at a constant temperature, were added dropwise to the vessel. The dropping rate of the two saturated solutions was controlled so that melamine and cyanuric acid were added dropwise to the reaction vessel at a molar ratio of 1:1. After the addition was completed, the temperature was kept constant until the reaction was completed. Then, the mixture was filtered, washed, and dried to obtain NaA molecular sieve raw powder with melamine cyanurate coated on the surface. The particle size of the NaA molecular sieve raw powder is 4 μm; The amino-containing silane coupling agent is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; The mass ratio of the NaA molecular sieve raw powder, deionized water, amino-containing silane coupling agent, and saturated melamine aqueous solution is 110:900:5:2800. The saturated melamine aqueous solution was added at a rate of 400 g / min; The reaction temperature is 80°C; Under the stirring condition, the stirring rate is 1100 rpm; After the reaction is complete, the reaction time is 3 hours; The temperature is maintained at a constant level until the reaction is complete, and the reaction time is 2 hours. The washing process involves washing twice with deionized water, with the mass of deionized water used in each wash being equal to the mass of the wet solid being washed. The drying process involves a drying temperature of 100°C and a drying time of 20 hours.
[0017] Step 2: Mixing and Molding NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, and deionized water are added to a double planetary mixer and stirred at high speed until initially mixed. Then, calcium peroxide powder is added and stirred at high speed until mixed a second time. Then, magnesium aluminum silicate is added and stirred at high speed until mixed a third time. The resulting viscous slurry is transferred into a granulator and formed into spherical particles. The silicate is potassium silicate; The calcium carbonate whiskers have a diameter of 1 μm and a length of 20 μm; The magnesium hydroxide whiskers have a diameter of 0.5 μm and a length of 13 μm; The kaolin has a particle size of 2 μm; The particle size of the calcium peroxide powder is 0.8 μm; The mass ratio of the NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, deionized water, calcium peroxide powder, and magnesium aluminum silicate is 280:30:25:20:30:800:15:3. The high-speed stirring has a stirring rate of 450 rpm. The initial mixing is uniform, and the mixing time is 5 hours; The secondary mixing process takes 1.6 hours. The three mixing processes are carried out over a period of 1 hour. The diameter of the spherical particles is 6 mm.
[0018] Step 3, roasting After the spherical particles were initially dried and solidified at 110℃ for 2 hours, they were then calcined at 600℃ for 5 hours at a rate of 4℃ / min, and then cooled to room temperature to obtain the calcined molecular sieve.
[0019] Step 4, Calcium Exchange The calcined molecular sieve was placed in a calcium chloride aqueous solution and exchanged at a constant temperature of 90°C for 4 hours. After filtration, the calcium-exchanged molecular sieve was obtained. The concentration of the calcium chloride aqueous solution is 0.5 mol / L; The mass ratio of the calcined molecular sieve to the calcium chloride aqueous solution is 10:53.
[0020] Step 5: Drying and Activation The calcium-exchanged molecular sieve was dried at 110℃ for 25 hours, and then activated at 650℃ for 3 hours at a heating rate of 3℃ / min to obtain 5A molecular sieve for pressure swing adsorption.
[0021] Example 2: A method for preparing 5A molecular sieves for pressure swing adsorption Step 1: Coating the surface of NaA molecular sieve powder NaA molecular sieve raw powder and deionized water were placed in a reaction vessel and heated to the reaction temperature while stirring. An amino-containing silane coupling agent was added at a constant temperature. After the reaction was complete, saturated melamine aqueous solution and saturated cyanuric acid aqueous solution, which were preheated to the reaction temperature and kept at a constant temperature, were added dropwise to the vessel. The dropping rate of the two saturated solutions was controlled so that melamine and cyanuric acid were added dropwise to the reaction vessel at a molar ratio of 1:1. After the addition was completed, the temperature was kept constant until the reaction was completed. Then, the mixture was filtered, washed, and dried to obtain NaA molecular sieve raw powder with melamine cyanurate coated on the surface. The particle size of the NaA molecular sieve raw powder is 2 μm; The amino-containing silane coupling agent is N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; The mass ratio of the NaA molecular sieve raw powder, deionized water, amino-containing silane coupling agent, and saturated melamine aqueous solution is 40:400:3:960. The saturated melamine aqueous solution was added at a rate of 120 g / min; The reaction temperature is 60°C; Under the specified stirring conditions, the stirring rate is 800 rpm; After the reaction is complete, the reaction time is 2 hours; The temperature is maintained at a constant level until the reaction is complete, and the reaction time is 1 hour. The washing process involves washing twice with deionized water, with the mass of deionized water used in each wash being equal to the mass of the wet solid being washed. The drying process involves a drying temperature of 85°C and a drying time of 24 hours.
[0022] Step 2: Mixing and Molding NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, and deionized water are added to a double planetary mixer and stirred at high speed until initially mixed. Then, calcium peroxide powder is added and stirred at high speed until mixed a second time. Then, magnesium aluminum silicate is added and stirred at high speed until mixed a third time. The resulting viscous slurry is transferred into a granulator and formed into spherical particles. The silicate is sodium metasilicate; The calcium carbonate whiskers have a diameter of 0.5 μm and a length of 8 μm. The magnesium hydroxide whiskers have a diameter of 0.1 μm and a length of 6 μm; The kaolin has a particle size of 0.2 μm; The particle size of the calcium peroxide powder is 0.1 μm; The mass ratio of the NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, deionized water, calcium peroxide powder, and magnesium aluminum silicate is 50:2:3:5:10:260:2:1. The high-speed stirring has a stirring rate of 300 rpm; The initial mixing is uniform, and the mixing time is 3 hours; The secondary mixing process takes 1 hour. The three mixing processes were carried out over a period of 0.6 hours. The diameter of the spherical particles is 2 mm.
[0023] Step 3, roasting After the spherical particles were initially dried and cured at 90℃ for 3.5 hours, they were then calcined at 500℃ for 6 hours at a rate of 3℃ / min. After cooling to room temperature, the calcined molecular sieve was obtained.
[0024] Step 4, Calcium Exchange The calcined molecular sieve was placed in a calcium chloride aqueous solution and exchanged at a constant temperature of 70°C for 7 hours. After filtration, the calcium-exchanged molecular sieve was obtained. The concentration of the calcium chloride aqueous solution is 0.1 mol / L; The mass ratio of the calcined molecular sieve to the calcium chloride aqueous solution is 10:33.
[0025] Step 5: Drying and Activation The calcium-exchanged molecular sieve was dried at 85°C for 35 hours, and then activated at 550°C for 4 hours at a heating rate of 1°C / min to obtain 5A molecular sieve for pressure swing adsorption.
[0026] Example 3: A method for preparing 5A molecular sieves for pressure swing adsorption Step 1: Coating the surface of NaA molecular sieve powder NaA molecular sieve raw powder and deionized water were placed in a reaction vessel and heated to the reaction temperature while stirring. An amino-containing silane coupling agent was added at a constant temperature. After the reaction was complete, saturated melamine aqueous solution and saturated cyanuric acid aqueous solution, which were preheated to the reaction temperature and kept at a constant temperature, were added dropwise to the vessel. The dropping rate of the two saturated solutions was controlled so that melamine and cyanuric acid were added dropwise to the reaction vessel at a molar ratio of 1:1. After the addition was completed, the temperature was kept constant until the reaction was completed. Then, the mixture was filtered, washed, and dried to obtain NaA molecular sieve raw powder with melamine cyanurate coated on the surface. The particle size of the NaA molecular sieve raw powder is 7 μm; The amino-containing silane coupling agent is N-(2-aminoethyl)-3-aminopropyltriethoxysilane; The mass ratio of the NaA molecular sieve raw powder, deionized water, amino-containing silane coupling agent, and saturated melamine aqueous solution is 130:1900:13:3800. The saturated melamine aqueous solution was added at a rate of 800 g / min; The reaction temperature is 85°C; Under the specified stirring conditions, the stirring rate is 1600 rpm; After the reaction is complete, the reaction time is 4.5 hours; The temperature was maintained at that level until the reaction was complete, and the reaction time was 3.5 hours. The washing process involves washing three times with deionized water, with the mass of deionized water used in each wash being equal to the mass of the wet solid being washed. The drying process is carried out at a temperature of 110°C for 15 hours.
[0027] Step 2: Mixing and Molding NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, and deionized water are added to a double planetary mixer and stirred at high speed until initially mixed. Then, calcium peroxide powder is added and stirred at high speed until mixed a second time. Then, magnesium aluminum silicate is added and stirred at high speed until mixed a third time. The resulting viscous slurry is transferred into a granulator and formed into spherical particles. The silicate is potassium silicate; The calcium carbonate whiskers have a diameter of 3 μm and a length of 30 μm; The magnesium hydroxide whiskers have a diameter of 1 μm and a length of 20 μm; The kaolin has a particle size of 6 μm; The particle size of the calcium peroxide powder is 1.3 μm; The mass ratio of the NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, deionized water, calcium peroxide powder, and magnesium aluminum silicate is 360:40:35:40:60:1000:25:5. The high-speed stirring has a stirring rate of 550 rpm. The initial mixing is uniform, and the mixing time is 6 hours; The secondary mixing process takes 2 hours. The three mixing processes take 1.5 hours. The diameter of the spherical particles is 7 mm.
[0028] Step 3, roasting After the spherical particles were initially dried and solidified at 130℃ for 1 hour, they were then calcined at 660℃ for 3 hours at a rate of 5℃ / min. After cooling to room temperature, the calcined molecular sieve was obtained.
[0029] Step 4, Calcium Exchange The calcined molecular sieve was placed in a calcium chloride aqueous solution and exchanged at a constant temperature of 95°C for 3 hours. After filtration, the calcium-exchanged molecular sieve was obtained. The concentration of the calcium chloride aqueous solution is 1 mol / L; The mass ratio of the calcined molecular sieve to the calcium chloride aqueous solution is 10:70.
[0030] Step 5: Drying and Activation The calcium-exchanged molecular sieve was dried at 130℃ for 15 hours, and then activated at 750℃ for 1.5 hours at a heating rate of 4℃ / min to obtain 5A molecular sieve for pressure swing adsorption.
[0031] Example 4: A method for preparing 5A molecular sieves for pressure swing adsorption Step 1: Coating the surface of NaA molecular sieve powder The amino-containing silane coupling agent is ureapropyltriethoxysilane, and the other operations are the same as in Example 1; Steps 2, 3, 4, and 5 are the same as in Example 1.
[0032] Comparative Example 1: Based on Example 1, without step 1 (coating the surface of the NaA molecular sieve powder), and in step 2 (mixing and molding), 280 parts of NaA molecular sieve powder coated with melamine cyanurate were replaced with an equal amount of NaA molecular sieve powder. The specific operation is as follows: Step 1, coating the surface of the NaA molecular sieve powder, is not performed; Step 2: Mixing and Molding Replace 280 parts of NaA molecular sieve raw powder coated with melamine cyanurate with an equal amount of NaA molecular sieve raw powder, and perform the other operations as in Example 1. The particle size of the NaA molecular sieve raw powder is 4 μm; Steps 3, 4, and 5 are the same as in Example 1.
[0033] Comparative Example 2: Based on Example 1, in step 2, mixing and molding, calcium carbonate whiskers were not added. Instead, 25 parts of calcium carbonate whiskers were replaced with 25 parts of deionized water. The specific operation is as follows: Step 1 is the same as in Example 1; Step 2: Mixing and Molding Replace 25 parts of calcium carbonate whiskers with 25 parts of deionized water, and perform the same operation as in Example 1. Steps 3, 4, and 5 are the same as in Example 1.
[0034] Comparative Example 3: Based on Example 1, in step 2, mixing and molding, magnesium hydroxide whiskers were not added. Instead, 20 parts of magnesium hydroxide whiskers were replaced with 20 parts of deionized water. The specific operation is as follows: Step 1 is the same as in Example 1; Step 2: Mixing and Molding Replace 20 parts of magnesium hydroxide whiskers with 20 parts of deionized water, and perform the other operations as in Example 1; Steps 3, 4, and 5 are the same as in Example 1.
[0035] Comparative Example 4: Based on Example 1, in step 2, mixing and molding, calcium peroxide powder was not added. Instead, 15 parts of calcium peroxide powder were replaced with 15 parts of deionized water. The specific operation is as follows: Step 1 is the same as in Example 1; Step 2: Mixing and Molding Replace 15 parts of calcium peroxide powder with 15 parts of deionized water, and perform the same operation as in Example 1. Steps 3, 4, and 5 are the same as in Example 1.
[0036] Performance testing: 1. Crushing resistance: The crushing resistance was tested in accordance with GB / T 13550-2015 5A molecular sieve and its test method and HGT 2783-2020 molecular sieve crushing resistance test method. 2. Wear rate: The wear rate was tested in accordance with "GB / T 13550-2015 5A molecular sieve and its determination method" and "GB / T 10504-2017 3A molecular sieve 5.2 Determination of wear rate". 3. Nitrogen adsorption performance: The adsorption capacity of nitrogen by 5A molecular sieve for pressure swing adsorption was tested using a Type II Mcbain vacuum adsorption instrument at 25°C and 1 standard atmosphere. Before the test, the vacuum was evacuated to 3 Pa and then cooled to 25°C. Nitrogen was then introduced into the test system. The adsorption capacity of the sample for nitrogen at adsorption equilibrium was tested at 25°C and 1 standard atmosphere. The test results are shown in Table 1: Table 1
[0037] As can be seen from the data in Table 1, the crushing resistance of Examples 1-4 is greater than 61.4 N, the abrasion rate is less than 0.16%, and the nitrogen adsorption capacity is above 21 mL / g. This indicates that the present invention has prepared a 5A molecular sieve for pressure swing adsorption with high adsorption capacity, high strength, and long service life. In Comparative Example 1, the surface of the NaA molecular sieve powder is not coated with melamine cyanurate. The crushing resistance and abrasion rate of Comparative Example 1 are almost the same as those of Example 1, but the nitrogen adsorption capacity of Comparative Example 1 is drastically reduced to 10.08 mL / g. This may be due to the melamine cyanurate coating. After urate coating of NaA molecular sieves, the thermal decomposition of melamine cyanurate during the calcination process forms numerous micropores on the surface of the NaA molecular sieve. These micropores provide ion exchange channels for subsequent calcium exchange, ensuring sufficient exchange between sodium and calcium ions in the NaA molecular sieve and enhancing the transformation of the NaA molecular sieve to the 5A molecular sieve crystal form. Furthermore, the micropores formed by the thermal decomposition of melamine cyanurate avoid the pore-clogging problem caused by the dense sintering of binders such as silicates and kaolin on the molecular sieve surface during calcination, thus increasing... The convenience and contact area between gas molecules and the molecular sieve particles during gas diffusion adsorption allow for sufficient contact between the ultrapores inside the molecular sieve particles and the adsorbed gas molecules. This is the fundamental reason why the 5A molecular sieve for pressure swing adsorption obtained in this invention has a very high nitrogen adsorption capacity. In Comparative Example 2, without the addition of calcium carbonate whiskers, the crushing resistance of Comparative Example 2 was significantly reduced, the wear rate was significantly increased, and the nitrogen adsorption capacity was also significantly reduced. This indicates that calcium carbonate whiskers play a crucial role in improving the mechanical properties of the molecular sieve, and the significant decrease in nitrogen adsorption capacity is evident in this. In terms of phenomena, calcium carbonate whiskers provide some support for the formation of micropores between molecular sieve particles during the calcination process. In Comparative Example 2, which does not contain calcium carbonate whiskers, the internal micropores are likely to collapse and become blocked during high-temperature sintering due to the loss of support. Consequently, there are not enough unobstructed micropores to promote gas diffusion into the surface of the molecular sieve particles, thus ultimately reducing the amount of gas adsorbed by the molecular sieve. In Comparative Example 3, which does not contain magnesium hydroxide whiskers, the crushing resistance of Comparative Example 3 increased to 74.7 N, and the wear rate decreased to 0.01%. This indicates that the addition of magnesium hydroxide whiskers significantly damages the mechanical properties of the molecular sieve. However, the nitrogen adsorption capacity of Comparative Example 3 also decreased significantly to 17%.57 The concentration of Mg(OH)2 / g may be due to the fact that the main function of magnesium hydroxide whiskers is to form large-sized through-pores through their own thermal decomposition during the calcination step. These pores have a certain negative impact on the mechanical properties of the molecular sieve, but the lack of these through-pores will also reduce the gas adsorption performance of the molecular sieve. In Comparative Example 4, no calcium peroxide powder was added. The crushing resistance of Comparative Example 4 was better than that of Example 1, and the wear rate was also lower than that of Example 1. This indicates that the addition of calcium peroxide powder has a certain degree of damage to the mechanical properties of the molecular sieve. The nitrogen adsorption capacity of Comparative Example 4 decreased significantly compared with Example 1. This may be because the thermal decomposition of calcium peroxide powder itself can play a role in pore formation. The micropores formed by the decomposition of calcium peroxide have a negative effect on mechanical properties, but have a very direct positive effect on gas adsorption performance. In addition, the calcium oxide formed by the thermal decomposition of calcium peroxide during the calcination step will generate calcium hydroxide in the calcium exchange step. The calcium ions released by the dissolution of calcium hydroxide can promote calcium exchange to a certain extent, thus increasing the calcium content in the final 5A molecular sieve for pressure swing adsorption. The increase in calcium content will greatly promote the improvement of the molecular sieve's nitrogen adsorption capacity. .
[0038] Appendix Figure 1 and attached Figure 2 The images show scanning electron microscope (SEM) images of the 5A molecular sieve for pressure swing adsorption obtained in Example 1, magnified 3000x and 6000x respectively. Both images clearly show numerous large pores ranging from micrometers to submicrometers distributed across the cross-section. These pores are mainly formed by the thermal decomposition of magnesium hydroxide whiskers and calcium peroxide powder, two pore-forming agents. These pores are interconnected, providing a rapid channel for gas diffusion into the interior of the 5A molecular sieve and facilitating rapid and sufficient contact between the surface of the 5A molecular sieve and the adsorbed gas molecules. Gas adsorption mainly occurs in the micropores inside the 5A molecular sieve particles. In addition, calcium carbonate whiskers can be seen interspersed in the dense sintered body of the molecular sieve in both images, providing mechanical support and effectively improving the overall mechanical properties of the molecular sieve.
[0039] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing 5A molecular sieves for pressure swing adsorption, characterized in that: The preparation method of the 5A molecular sieve for pressure swing adsorption includes five steps: coating the surface of NaA molecular sieve raw powder, mixing and molding, calcination, calcium exchange, and drying and activation. The surface of the NaA molecular sieve powder is coated by placing the NaA molecular sieve powder and deionized water into a reaction vessel, heating it to the reaction temperature while stirring, adding an amino-containing silane coupling agent at a constant temperature, and after the reaction is complete, simultaneously adding a saturated melamine aqueous solution and a saturated cyanuric acid aqueous solution preheated to the reaction temperature and kept at a constant temperature into the vessel. The dropping rate of the two saturated solutions is controlled so that melamine and cyanuric acid are added to the reaction vessel in a molar ratio of 1:
1. After the addition is complete, the temperature is kept constant until the reaction is complete, and then filtered, washed, and dried to obtain NaA molecular sieve powder with melamine cyanurate coated on the surface. The amino-containing silane coupling agent is at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and ureapropyltriethoxysilane. The mixing and molding process involves adding NaA molecular sieve powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, and deionized water to a double planetary mixer. After high-speed mixing until initially homogeneous, calcium peroxide powder is added, and high-speed mixing continues until homogeneous a second time. Then, magnesium aluminum silicate is added, and high-speed mixing continues until homogeneous a third time. The resulting viscous slurry is then transferred into a granulator to form spherical particles.
2. The method for preparing 5A molecular sieve for pressure swing adsorption according to claim 1, characterized in that: The calcination process involves placing the spherical particles at a temperature of 90-130°C for initial drying and solidification for 1-3.5 hours, then calcining them at a temperature of 500-660°C for 3-6 hours at a rate of 3-5°C / min, and finally cooling them to room temperature to obtain the calcined molecular sieve. The calcium exchange involves placing the calcined molecular sieve into a calcium chloride aqueous solution and exchanging it at a constant temperature of 70-95°C for 3-7 hours, followed by filtration to obtain the calcium-exchanged molecular sieve. The drying and activation process involves drying the calcium-exchanged molecular sieve at 85-130°C for 15-35 hours, and then activating it at 550-750°C for 1.5-4 hours at a heating rate of 1-4°C / min to obtain 5A molecular sieve for pressure swing adsorption.
3. The method for preparing 5A molecular sieve for pressure swing adsorption according to claim 1, characterized in that: The particle size of the NaA molecular sieve raw powder is 2~7μm; The mass ratio of the NaA molecular sieve raw powder, deionized water, amino-containing silane coupling agent, and saturated melamine aqueous solution is 40~130:400~1900:3~13:960~3800; The saturated melamine aqueous solution is added at a rate of 120-800 g / min.
4. The method for preparing 5A molecular sieve for pressure swing adsorption according to claim 1, characterized in that: The silicate is at least one of potassium silicate and sodium metasilicate; The calcium carbonate whiskers have a diameter of 0.5~3μm and a length of 8~30μm; The magnesium hydroxide whiskers have a diameter of 0.1~1μm and a length of 6~20μm; The kaolin has a particle size of 0.2~6μm; The particle size of the calcium peroxide powder is 0.1~1.3μm; The mass ratio of the NaA molecular sieve raw powder coated with melamine cyanurate, silicate, calcium carbonate whiskers, magnesium hydroxide whiskers, kaolin, deionized water, calcium peroxide powder, and magnesium aluminum silicate is 50~360:2~40:3~35:5~40:10~60:260~1000:2~25:1~5.
5. The 5A molecular sieve for pressure swing adsorption prepared by any one of the preparation methods according to claims 1-4, characterized in that: The 5A molecular sieve used for pressure swing adsorption has a crushing force of 61.4~67.9N, an abrasion rate of 0.08~0.16%, and a nitrogen adsorption capacity of 21.45~24.83mL / g.
Citation Information
Patent Citations
Preparation method of 5A molecular sieve adsorbent
CN114433014A
Preparation method of 5A molecular sieve adsorbent
CN114682237A