Scrimber with sandwich structure
By adopting a sandwich sandwich structure in the recombinant material, using surface and core layers of different densities and glue application amounts, combined with dispersion and hot pressing processes, the problem of insufficient performance of the existing recombinant material is solved, significantly improving the strength and stability of the material sex.
Patent Information
- Application Number
- CN202323632408.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2033-12-29
AI Technical Summary
The uniform material structure of existing recombinant materials is difficult to meet the needs of lightweight, high strength, high hardness and high dimensional stability, especially in the process of expanding their application areas.
A recombinant material design adopts a sandwich sandwich structure, in which the upper and lower surface layers and core layers have different densities, fiber bundle diameters and glue application amounts, and a dislocation interface is formed through disassembly, drying, glue application and hot pressing processes to improve material performance.
Through the setting of fiber bundles of different diameters, glue application amounts and hot pressing processes, the strength, surface hardness, dimensional stability and wear resistance of the recombinant material are improved.
Smart Images

Figure CN222003831U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of wood processing, and in particular relates to a reconstituted material with a sandwich core structure. Background Art
[0002] Recombinant materials mainly include recombinant bamboo and recombinant wood, which are boards or square materials made by processing wood or bamboo into wooden recombinant units or bamboo recombinant units, impregnating them with resin, and then drying, adjusting temperature and humidity, paving, hot pressing and other processes. Existing recombinant materials are usually made of uniform materials, with the same parameters such as fiber bundle diameter, glue application amount, and moisture content. The surface layer and core layer of the manufactured recombinant materials have the same density, which makes it difficult to give full play to the advantages and characteristics of recombinant materials. With the expansion of the application field of recombinant materials, new requirements have been put forward for light weight, high strength, high hardness and high dimensional stability, which are difficult to meet with existing recombinant materials. To this end, the utility model proposes a recombinant material with a sandwich structure. Utility Model Content
[0003] In order to solve the above problems, the utility model proposes a recombinant material with a sandwich structure.
[0004] In order to achieve the above purpose, the utility model provides the following technical solutions:
[0005] A recombinant material with a sandwich structure, comprising an upper surface layer, a lower surface layer and a core layer, wherein the surface layer density is 1.15-1.35 g / cm 3 ; The core layer density is 0.65-1.25g / cm 3 The core layer is located between the upper and lower surface layers to form a sandwich structure.
[0006] The core layer density is 0.85-1.15 g / cm 3 .
[0007] The thickness of the upper and lower surface layers is respectively 15-40% of the thickness of the recombinant material, and the thickness of the core layer is 30-70% of the thickness of the recombinant material.
[0008] The surface layer recombinant unit and the core layer recombinant unit have a certain misalignment on the bonding interface, and the misalignment height is ≥2mm and ≤10mm.
[0009] The average diameter of the fiber bundle of the surface layer reorganization unit is ≤2.5mm, and the maximum diameter is ≤3.0mm; the average diameter of the fiber bundle of the core layer reorganization unit is ≤3.5mm, and the maximum diameter is ≤4.5mm.
[0010] The glue application amount of the surface layer recombinant unit is 8-25%; the glue application amount of the core layer recombinant unit is 5-20%.
[0011] More specifically, the method for preparing the recombinant material having a sandwich structure comprises the following steps:
[0012] (1) Preparation of recombinant units
[0013] Preparation of surface recombinant units: bamboo or wood is deflaked into wood or bamboo recombinant units with an average fiber bundle diameter of ≤2.5 mm and a maximum fiber bundle diameter of ≤3.0 mm using a special deflaking device;
[0014] Preparation of core layer recombinant units: bamboo or wood is deflaked into wood or bamboo recombinant units with an average fiber bundle diameter of ≤3.5 mm and a maximum fiber bundle diameter of ≤4.5 mm using a special deflaking device;
[0015] (2) Primary drying of the reorganization unit
[0016] The prepared surface layer recombinant unit is dried by drying equipment to a moisture content of 3-8% at a drying temperature of 90-110°C; the prepared core layer recombinant unit is dried by drying equipment to a moisture content of 3-8% at a drying temperature of 90-110°C;
[0017] (3) Recombination unit sizing
[0018] The surface reconstructed unit after the primary drying is dipped into or rolled with phenolic resin, with the glue amount being 8-25%; the core reconstructed unit after the primary drying is dipped into or rolled with phenolic resin, with the glue amount being 5-20%;
[0019] (4) Secondary drying of the recombination unit
[0020] The prepared pre-impregnated surface layer reorganization unit is dried by a drying device until the moisture content is 15-25% and the drying temperature is 55-65°C; the prepared pre-impregnated core layer reorganization unit is dried by a drying device until the moisture content is 8-15% and the drying temperature is 55-75°C;
[0021] (5) Recombination unit balance processing
[0022] The surface reorganization units after secondary drying are subjected to balancing treatment in a balancing room or storage bin until the moisture content is 15-25%, and the moisture content deviation between the surface reorganization units is controlled within 5%;
[0023] The core layer reorganization unit after secondary drying is subjected to balancing treatment in a balancing room or storage bin to a moisture content of 8-15%, and the moisture content deviation between the core layer reorganization units is controlled within 5%;
[0024] (6) Recombination unit assembly
[0025] The mass ratio of the surface layer recombinant unit to the core layer recombinant unit is 1:2-2:1;
[0026] The secondary dried surface reorganization unit is evenly divided into two parts, one of which is laid flat on the laying table along the grain as the lower surface layer, and the secondary dried core layer reorganization unit is laid flat on the lower surface layer reorganization unit along the grain, and then the other secondary dried surface layer reorganization unit is laid flat on the core layer reorganization unit along the grain to complete the assembly;
[0027] (7) Hot pressing of recombinant materials
[0028] The laid reconstituted material slab is sent into a hot press for hot pressing. The forming process is as follows: hot pressing temperature 120-140°C, hot pressing time 30-150 minutes, hot pressing pressure 5-15MPa, and the sandwich core structure reconstituted material can be obtained.
[0029] Compared with the prior art, the utility model has the following advantages and technical effects:
[0030] The utility model prepares a recombinant material with a sandwich core structure by setting fiber bundles of different diameters, different sizing amounts, moisture contents and hot pressing processes, thereby improving the strength, surface hardness, dimensional stability and wear resistance of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings that constitute part of this application are used to provide a further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute an improper limitation on this application. In the drawings:
[0032] Figure 1 It is a schematic structural diagram of a recombinant material with a sandwich structure according to the utility model;
[0033] Figure 2 It is the bonding interface of the surface and core layers of the new recombinant material of the utility model, wherein h is the dislocation difference of the recombinant unit. DETAILED DESCRIPTION
[0034] Various exemplary embodiments of the present invention are now described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features and embodiments of the present invention.
[0035] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0036] Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art in the field of the utility model. Although the utility model only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the utility model. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention will be apparent to those skilled in the art. The present invention description and examples are merely exemplary.
[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0039] Example 1
[0040] The sandwich structure of the bamboo reconstructed bamboo includes an upper surface layer, a lower surface layer and a core layer, and the surface layer density is 1.35g / cm 3 , core layer density is 1.15g / cm 3 The thickness of the upper and lower surface layers is 6mm, the thickness of the core layer is 15mm, the offset height of the surface layer reorganization unit and the core layer reorganization unit at the bonding interface is 3.0mm, the average diameter of the fiber bundle of the surface layer reorganization unit is 2.0mm, and the maximum diameter is 3.0mm; the average diameter of the fiber bundle of the core layer reorganization unit is 3.0mm, and the maximum diameter is 4.5mm. The core layer is located between the upper and lower surface layers to form a sandwich structure. The specific preparation method is as follows:
[0041] (1) Preparation of recombinant units
[0042] Preparation of surface recombinant units: bamboo materials are decomposed into bamboo recombinant units with an average fiber bundle diameter of 2.0 mm and a maximum fiber bundle diameter of 3.0 mm using a special decomposition device;
[0043] Preparation of core layer recombinant units: bamboo materials are decomposed into bamboo recombinant units with an average fiber bundle diameter of 3.0 mm and a maximum fiber bundle diameter of 4.5 mm using a special decomposition device;
[0044] (2) Primary drying of the reorganization unit
[0045] The prepared surface layer recombinant unit is dried by a drying device until the moisture content is 8% and the drying temperature is 90°C; the prepared core layer recombinant unit is dried by a drying device until the moisture content is 8% and the drying temperature is 90°C;
[0046] (3) Recombination unit sizing
[0047] The surface layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 25%; the core layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 12%;
[0048] (4) Secondary drying of the recombination unit
[0049] The prepared pre-impregnated surface layer reorganization unit is dried by a drying device to a moisture content of 25% and a drying temperature of 55°C; the prepared pre-impregnated core layer reorganization unit is dried by a drying device to a moisture content of 12% and a drying temperature of 55°C;
[0050] (5) Recombination unit balance processing
[0051] The surface reorganization units after secondary drying are subjected to balancing treatment in a balancing room or storage bin until the moisture content is 25%, and the moisture content deviation between the surface reorganization units is controlled within 5%;
[0052] The core layer reorganization unit after secondary drying is subjected to balancing treatment in a balancing room or storage bin until the moisture content is 12%, and the moisture content deviation between the core layer reorganization units is controlled within 5%;
[0053] (6) Recombination unit assembly
[0054] The mass ratio of the surface layer recombinant unit to the core layer recombinant unit is 0.75;
[0055] The secondary dried surface reorganization unit is evenly divided into two parts, one of which is laid flat on the laying table along the grain as the lower surface layer, and the secondary dried core layer reorganization unit is laid flat on the lower surface layer reorganization unit along the grain, and then the other secondary dried surface layer reorganization unit is laid flat on the core layer reorganization unit along the grain to complete the assembly;
[0056] (7) Hot pressing of recombinant materials
[0057] The laid reconstructed material slab is sent into a hot press for hot pressing. The molding process is as follows: hot pressing temperature of 140° C., hot pressing time of 45 minutes, and hot pressing pressure of 10 MPa, so as to obtain the moso bamboo reconstructed bamboo with a sandwich structure.
[0058] Example 2
[0059] The poplar wood with sandwich structure includes upper surface layer, lower surface layer and core layer, and the surface layer density is 1.15g / cm 3, core layer density is 0.65g / cm 3 The thickness of the upper and lower surface layers is 5mm, the thickness of the core layer is 10mm, the offset height of the surface layer reorganization unit and the core layer reorganization unit at the bonding interface is 2.0mm, the average diameter of the fiber bundle of the surface layer reorganization unit is 1.5mm, and the maximum diameter is 2.5mm; the average diameter of the fiber bundle of the core layer reorganization unit is 2.0mm, and the maximum diameter is 2.5mm. The core layer is located between the upper and lower surface layers to form a sandwich structure. The specific preparation method is as follows:
[0060] (1) Preparation of recombinant units
[0061] Preparation of surface recombinant units: Poplar wood is decomposed into wood recombinant units with an average fiber bundle diameter of 1.5 mm and a maximum fiber bundle diameter of 2.5 mm using a special decomposition device;
[0062] Preparation of core layer recombinant units: Poplar wood is decomposed into wood recombinant units with an average fiber bundle diameter of 2.0 mm and a maximum fiber bundle diameter of 2.5 mm using a special decomposition device;
[0063] (2) Primary drying of the reorganization unit
[0064] The prepared surface layer recombinant unit is dried by a drying device to a moisture content of 5.0% at a drying temperature of 110°C; the prepared core layer recombinant unit is dried by a drying device to a moisture content of 5.0% at a drying temperature of 110°C;
[0065] (3) Recombination unit sizing
[0066] The surface layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 25%; the core layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 12%;
[0067] (4) Secondary drying of the recombination unit
[0068] The prepared pre-impregnated surface layer reorganization unit is dried by a drying device to a moisture content of 15% and a drying temperature of 65°C; the prepared pre-impregnated core layer reorganization unit is dried by a drying device to a moisture content of 8% and a drying temperature of 65°C;
[0069] (5) Recombination unit balance processing
[0070] The surface reorganization units after secondary drying are subjected to balancing treatment in a balancing room or storage bin until the moisture content is 15%, and the moisture content deviation between the surface reorganization units is controlled within 5%;
[0071] The core layer reorganization unit after secondary drying is subjected to balancing treatment in a balancing room or storage bin to a moisture content of 8%, and the moisture content deviation between the core layer reorganization units is controlled within 5%;
[0072] (6) Recombination unit assembly
[0073] The mass ratio of the surface layer recombinant unit to the core layer recombinant unit is 1.75;
[0074] The secondary dried surface reorganization unit is evenly divided into two parts, one of which is laid flat on the laying table along the grain as the lower surface layer, and the secondary dried core layer reorganization unit is laid flat on the lower surface layer reorganization unit along the grain, and then the other secondary dried surface layer reorganization unit is laid flat on the core layer reorganization unit along the grain to complete the assembly;
[0075] (7) Hot pressing of recombinant materials
[0076] The laid reconstituted material slab is sent into a hot press for hot pressing molding. The molding process is as follows: hot pressing temperature 140° C., hot pressing time 30 minutes, hot pressing pressure 5 MPa, and the poplar reconstituted wood with a sandwich structure can be obtained.
[0077] Example 3
[0078] The eucalyptus reconstituted wood with sandwich structure includes upper surface layer, lower surface layer and core layer, and the surface layer density is 1.35g / cm 3 , core layer density is 0.85g / cm 3 The thickness of the upper and lower surface layers is 5mm, the thickness of the core layer is 20mm, the offset height of the surface layer reorganization unit and the core layer reorganization unit at the bonding interface is 4.5mm, the average diameter of the fiber bundle of the surface layer reorganization unit is 1.5mm, and the maximum diameter is 2.5mm; the average diameter of the fiber bundle of the core layer reorganization unit is 3.5mm, and the maximum diameter is 4.5mm. The core layer is located between the upper and lower surface layers to form a sandwich structure. The specific preparation method is as follows:
[0079] (1) Preparation of recombinant units
[0080] Preparation of surface recombinant units: Eucalyptus wood is deflaked into wood recombinant units with an average fiber bundle diameter of 1.5 mm and a maximum fiber bundle diameter of 2.5 mm using a special deflaking device;
[0081] Preparation of core layer recombinant units: Eucalyptus wood is deflaked into wood recombinant units with an average fiber bundle diameter of 3.5 mm and a maximum fiber bundle diameter of 4.5 mm using a special deflaking device;
[0082] (2) Primary drying of the reorganization unit
[0083] The prepared surface layer recombinant unit is dried by a drying device until the moisture content is 3.0% and the drying temperature is 100°C; the prepared core layer recombinant unit is dried by a drying device until the moisture content is 3.0% and the drying temperature is 100°C;
[0084] (3) Recombination unit sizing
[0085] The surface layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 25%; the core layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 8%;
[0086] (4) Secondary drying of the recombination unit
[0087] The prepared pre-impregnated surface layer reorganization unit is dried by a drying device to a moisture content of 25% and a drying temperature of 65°C; the prepared pre-impregnated core layer reorganization unit is dried by a drying device to a moisture content of 6% and a drying temperature of 65°C;
[0088] (5) Recombination unit balance processing
[0089] The surface reorganization units after secondary drying are subjected to balancing treatment in a balancing room or storage bin until the moisture content is 25%, and the moisture content deviation between the surface reorganization units is controlled within 5%;
[0090] The core layer reorganization unit after secondary drying is subjected to balancing treatment in a balancing room or storage bin to a moisture content of 6%, and the moisture content deviation between the core layer reorganization units is controlled within 5%;
[0091] (6) Recombination unit assembly
[0092] The mass ratio of the surface layer recombinant unit to the core layer recombinant unit is 0.80;
[0093] The secondary dried surface reorganization unit is evenly divided into two parts, one of which is laid flat on the laying table along the grain as the lower surface layer, and the secondary dried core layer reorganization unit is laid flat on the lower surface layer reorganization unit along the grain, and then the other secondary dried surface layer reorganization unit is laid flat on the core layer reorganization unit along the grain to complete the assembly;
[0094] (7) Hot pressing of recombinant materials
[0095] The laid reconstituted wood slab is sent into a hot press for hot pressing. The forming process is as follows: hot pressing temperature of 140° C., hot pressing time of 60 minutes, and hot pressing pressure of 15 MPa, so as to obtain the eucalyptus reconstituted wood with a sandwich structure.
[0096] Example 4
[0097] The sandwich structure of rubber wood reconstituted wood includes an upper surface layer, a lower surface layer and a core layer, and the surface layer density is 1.25g / cm 3 , core layer density is 0.85g / cm 3The thickness of the upper and lower surface layers is 15mm, the thickness of the core layer is 25mm, the offset height of the surface layer reorganization unit and the core layer reorganization unit at the bonding interface is 10.0mm, the average diameter of the fiber bundle of the surface layer reorganization unit is 1.2mm, and the maximum diameter is 1.5mm; the average diameter of the fiber bundle of the core layer reorganization unit is 3.0mm, and the maximum diameter is 3.5mm. The core layer is located between the upper and lower surface layers to form a sandwich structure. The specific preparation method is as follows:
[0098] (1) Preparation of recombinant units
[0099] Preparation of surface recombinant units: Rubber wood is decomposed into wood recombinant units with an average fiber bundle diameter of 1.2 mm and a maximum fiber bundle diameter of 1.5 mm using a special decomposition device;
[0100] Preparation of core layer recombinant unit: Rubber wood is decomposed into wood recombinant units with an average fiber bundle diameter of 3.0 mm and a maximum fiber bundle diameter of 3.5 mm by using a special decomposition device;
[0101] (2) Primary drying of the reorganization unit
[0102] The prepared surface layer recombinant unit is dried by a drying device until the moisture content is 8.0% and the drying temperature is 110°C; the prepared core layer recombinant unit is dried by a drying device until the moisture content is 8.0% and the drying temperature is 110°C;
[0103] (3) Recombination unit sizing
[0104] The surface layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 10%; the core layer reorganization unit after the primary drying is impregnated with phenolic resin, and the sizing amount is 10%;
[0105] (4) Secondary drying of the recombination unit
[0106] The prepared pre-impregnated surface layer reorganization unit is dried by a drying device to a moisture content of 20% and a drying temperature of 65°C; the prepared pre-impregnated core layer reorganization unit is dried by a drying device to a moisture content of 8% and a drying temperature of 65°C;
[0107] (5) Recombination unit balance processing
[0108] The surface reorganization units after secondary drying are subjected to balancing treatment in a balancing room or storage bin until the moisture content is 20%, and the moisture content deviation between the surface reorganization units is controlled within 5%;
[0109] The core layer reorganization unit after secondary drying is subjected to balancing treatment in a balancing room or storage bin to a moisture content of 8%, and the moisture content deviation between the core layer reorganization units is controlled within 5%;
[0110] (6) Recombination unit assembly
[0111] The mass ratio of the surface layer recombinant unit to the core layer recombinant unit is 1.75;
[0112] The secondary dried surface reorganization unit is evenly divided into two parts, one of which is laid flat on the laying table along the grain as the lower surface layer, and the secondary dried core layer reorganization unit is laid flat on the lower surface layer reorganization unit along the grain, and then the other secondary dried surface layer reorganization unit is laid flat on the core layer reorganization unit along the grain to complete the assembly;
[0113] (7) Hot pressing of recombinant materials
[0114] The laid reconstituted material slab is sent into a hot press for hot pressing molding. The molding process is as follows: hot pressing temperature of 140° C., hot pressing time of 90 minutes, and hot pressing pressure of 8 MPa, so as to obtain the rubber wood reconstituted wood with a sandwich structure.
[0115] The performance tests were conducted on the novel bamboo recombinant materials prepared in Examples 1 to 4. The test results are shown in Table 1, wherein the performance test standards are as follows:
[0116] Elastic modulus: measured in accordance with GB / T 17657-2022
[0117] Static bending strength: measured in accordance with GB / T 17657-2022
[0118] Horizontal shear strength: measured in accordance with GB / T 30364-2013
[0119] Water absorption thickness expansion rate: measured in accordance with GB / T 30364-2013
[0120] Table 1 Performance of recombinant materials prepared in Examples 1 to 4
[0121]
[0122] It can be seen from Table 1 that the physical and mechanical properties of the reconstituted materials prepared in Examples 1 to 4 can all meet the physical and mechanical performance indicators of "Reconstituted Bamboo Flooring" GB / T 30364-2013.
[0123] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A recombinant material with a sandwich structure, characterized in that: It includes an upper surface layer, a lower surface layer and a core layer, wherein the surface layer density is 1.15-1.35 g / cm 3 ; The core layer density is 0.65-1.25g / cm 3 The core layer is located between the upper and lower surface layers to form a sandwich structure.
2. The recombinant material with a sandwich structure according to claim 1, characterized in that: The core layer density is 0.85-1.15 g / cm 3 .
3. The recombinant material with a sandwich structure according to claim 1, characterized in that: The thickness of the upper and lower surface layers is respectively 15-40% of the thickness of the recombinant material, and the thickness of the core layer is 30-70% of the thickness of the recombinant material.
4. The recombinant material with a sandwich structure according to claim 1, characterized in that: The surface layer recombinant unit and the core layer recombinant unit have a misalignment height at the bonding interface, and the misalignment height is ≥2mm and ≤10mm.
5. The recombinant material with a sandwich structure according to claim 1, characterized in that: The average diameter of the fiber bundle of the surface layer reorganization unit is ≤2.5mm, and the maximum diameter is ≤3.0mm; the average diameter of the fiber bundle of the core layer reorganization unit is ≤3.5mm, and the maximum diameter is ≤4.5mm.