Copper fine particle and copper fine particle production method
Copper fine particles coated with terpineol and dodecylamine address the limitations of traditional bonding materials by providing oxidation resistance and heat dissipation, enabling effective bonding and conductivity in high-temperature applications for power semiconductor devices.
Patent Information
- Application Number
- PCT/JP2024/012037
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Current bonding materials, such as solder, are inadequate for high-temperature applications of power semiconductor devices using wide bandgap semiconductors, as they melt at operating temperatures, restricting device usage and requiring oxidation-resistant metal fine particles that maintain conductivity and heat dissipation.
Copper fine particles coated with terpineol and dodecylamine, with particle sizes between 10 to 100 nm, are produced using a thermal plasma method, providing excellent oxidation resistance in both air and moist environments, enabling stable storage and high-temperature bonding.
The copper fine particles exhibit superior oxidation resistance and heat dissipation, allowing for reliable bonding and conductivity in high-temperature environments, suitable for power semiconductor devices and other heat-generating applications.
Smart Images

Figure JP2024012037_03102024_PF_FP_ABST
Abstract
Description
Copper microparticles and method for producing copper microparticles
[0001] The present invention relates to copper microparticles and a method for producing copper microparticles used for bonding semiconductor elements, high-frequency devices, light-emitting diodes, semiconductor lasers, etc. to substrates, etc., and in particular to copper microparticles and a method for producing copper microparticles that take into consideration oxidation inhibition.
[0002] Currently, power semiconductor elements using wide-bandgap semiconductors such as silicon carbide (SiC), gallium nitride (GaN), gallium oxide, or diamond are being developed. Compared to semiconductor elements using Si or GaAs, power semiconductor elements have lower on-resistance, enable high-speed switching, and can be miniaturized. Furthermore, power semiconductor elements have high heat resistance and can operate at high temperatures of 250-300°C. Solder has traditionally been used to bond semiconductor elements to substrates, etc. However, power semiconductor elements operate at higher temperatures than conventional semiconductor elements using Si or GaAs, and solder bonding requires them to be used at temperatures below the melting point of the solder. When solder is used as a bonding material, power semiconductor elements must be used at temperatures below the melting point of the solder, which places limitations on their use. Thus, bonding materials are also required to be able to be used at high temperatures. For example, bonding materials include pastes in which metal particles are dispersed in a solvent. The smaller the metal particles, the larger their specific surface area and the more susceptible they are to oxidation. For this reason, for example, Patent Document 1 proposes a method for suppressing oxidation of metal fine particles.
[0003] Patent Document 1 describes a bonding material particle having an organic protective film formed on the surface of copper nanoparticles, the bonding material particle having a BET specific surface area of 3.5 m 2 / g or more 8m 2 / g or less, the BET diameter converted from the specific surface area is in the range of 80 nm or more and 200 nm or less, the organic protective film is contained in the range of 0.5 mass % or more and 2.0 mass % or less with respect to 100 mass % of the particles for the bonding material, and when the particles for the bonding material are analyzed using time-of-flight secondary ion mass spectrometry (TOF-SIMS), C 3 H 3 O 3 -Ion and C 3 H 4 O 2 - The detected amount of each ion is Cu + The amount of the ion detected is in the range of 0.05 to 0.2 times, and C 5 The amount of detected ions is Cu + The amount of the ion detected is less than 0.005 times the amount of the ion detected. The organic protective film is a film derived from citric acid. Patent Document 1 also describes a bonding paste containing bonding material particles.
[0004] Japanese Patent Application Laid-Open No. 2020-59914
[0005] In Patent Document 1, copper nanoparticles are coated with an organic protective film to suppress oxidation during storage. However, for example, as described above, a paste in which bonding material particles are dispersed in a solvent is used as the bonding material. Therefore, it is necessary to suppress oxidation not only during storage but also when dispersed in a solvent, etc. In particular, when the paste contains moisture, the small size of the metal microparticles increases the specific surface area, making them more susceptible to oxidation. Thus, it is necessary to consider not only the oxidation resistance of the metal microparticles in the atmosphere at room temperature where they are stored, but also the oxidation resistance of the metal microparticles in a humid environment, such as when they are made into a paste. However, currently, there are no bonding materials that have been studied to address both of these oxidation resistances. Furthermore, it is desirable to easily impart oxidation resistance to metal microparticles.
[0006] An object of the present invention is to provide copper microparticles that are excellent in suppressing oxidation in the atmosphere at room temperature and in a humid environment, and a method for producing copper microparticles in a simple manner.
[0007] In order to achieve the above object, one aspect of the present invention provides copper microparticles whose surfaces are coated with terpineol and dodecylamine and whose particle diameters measured by the BET method are 10 to 100 nm. -3 g / m 2 The amount of dodecylamine introduced per unit area is preferably 1.20 × 10 -4 g / m 2The amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is preferably 1.48 × 10 -3 g / m 2 It is preferable that this is equal to or greater than this.
[0008] One aspect of the present invention is a method for producing copper microparticles, which includes the steps of: supplying a carrier gas in which copper powder is dispersed into a thermal plasma flame, and then supplying a cooling gas to the end of the thermal plasma flame to generate microparticles; and supplying a surface treatment agent containing terpineol and dodecylamine to the microparticles in an air-dispersed state before the microparticles are collected, in a temperature range where the surface treatment agent is not denatured. The amount of terpineol introduced per unit area is 1.36 × 10 -3 g / m 2 The amount of dodecylamine introduced per unit area is preferably 1.20 × 10 -4 g / m 2 The amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is preferably 1.48 × 10 -3 g / m 2 The cooling gas is preferably argon gas, helium gas, or nitrogen gas. The plasma gas of the thermal plasma flame is preferably argon gas, helium gas, hydrogen gas, or nitrogen gas.
[0009] According to the present invention, it is possible to provide copper microparticles that are excellent in suppressing oxidation in the air at room temperature and in a humid environment, and a method for producing copper microparticles in a simple manner.
[0010] It is a schematic diagram showing an example of a use form of copper fine particles of the present invention. It is a schematic diagram showing another example of a use form of copper fine particles of the present invention. It is a schematic diagram showing an example of a manufacturing apparatus for copper fine particles of the present invention.
[0011] The copper microparticles and the method for producing copper microparticles of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings. Note that the drawings described below are illustrative for explaining the present invention and are simplified for explaining the present invention. Therefore, the present invention is not limited to the drawings shown below. Note that in the following, the term "to" indicating a numerical range includes the numerical values written on both sides. For example, when ε is a numerical value ε α ~Number ε β That is, the range of ε is the number ε α and the number ε β The range includes ε α ≦ε≦ε β In addition, unless otherwise specified, various numerical values include error ranges generally accepted in the relevant technical field. Copper microparticles and a method for producing copper microparticles will be described below.
[0012] [Example of Copper Fine Particles] The copper fine particles have a surface coated with terpineol and dodecylamine, and have a particle size measured by the BET method of 10 to 100 nm.
[0013] Terpineol (C 10 H 18 O) exhibits oxidation resistance in the atmosphere at room temperature. Terpineol is a type of monoterpene alcohol, also known as terpineol.
[0014] Here, the atmosphere refers to what is commonly called air. The composition of the atmosphere, i.e., the composition of air, is 78.08% by volume of nitrogen, 20.95% by volume of oxygen, 0.93% by volume of argon, and 0.03% by volume of carbon dioxide. Note that a general measurement error is allowed for the air composition. The room temperature is 25°C.
[0015] Dodecylamine exhibits oxidation resistance against moisture. Furthermore, dodecylamine exhibits oxidation resistance against air at room temperature, although this is inferior to that of terpineol. Dodecylamine has a linear chain structure. The presence or absence of surface coating on copper microparticles and the composition of terpineol and dodecylamine can be investigated using, for example, an FT-IR (Fourier transform infrared spectrophotometer).
[0016] In copper microparticles whose surfaces are coated with terpineol and dodecylamine, the terpineol and dodecylamine must be present to entirely or partially cover the surface of the copper microparticles. If the terpineol and dodecylamine are not present to entirely or partially cover the surface of the copper microparticles, the oxidation resistance of the copper microparticles to the air at room temperature and to moisture described above may not be fully exhibited, and it may be difficult to obtain the oxidation suppression effect.
[0017] In the copper fine particles, the amount of terpineol introduced per unit area is 1.36 × 10 -3 g / m 2 The amount of terpineol introduced per unit area is preferably 1.36 × 10 or more. -3 g / m 2 If the amount is more than this, the copper fine particles can sufficiently exhibit oxidation resistance in the atmosphere at room temperature. -1 g / m 2 In addition, the amount of dodecylamine introduced per unit area of the copper particles is 1.20 × 10 -4 g / m 2 Furthermore, it is preferable that the amount of dodecylamine introduced per unit area is 3.55×10 or more. -3 g / m 2 If the amount is equal to or greater than this, the copper fine particles can exhibit sufficient oxidation resistance against moisture and also exhibit sufficient oxidation resistance against the atmosphere at room temperature. -2 g / m 2 In addition, in the copper microparticles, the amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is 1.48 × 10 -3 g / m 2 The total amount of terpineol and dodecylamine introduced per unit area is preferably 1.48 × 10 or more. -3 g / m 2If the amount is more than this, the copper fine particles can sufficiently exhibit oxidation resistance to the atmosphere at room temperature and oxidation resistance to moisture. -1 g / m 2 is.
[0018] Furthermore, the copper microparticles have a particle size of 10 to 100 nm, preferably 30 to 90 nm, as measured by the BET method as described above. The particle size of the copper microparticles described above is an average particle size measured using the BET method. In the BET method, the particle size is calculated from the specific surface area, assuming that the particles are spherical. To measure the particle size of the copper microparticles, a Macsorb HM-1208 (trade name) manufactured by Mountech Co., Ltd. is used. The particle size of the copper microparticles described above is the particle size when the surface is coated with terpineol and dodecylamine.
[0019] The copper microparticles have a surface coated with terpineol and dodecylamine, for example, a coating layer (not shown) composed of terpineol and dodecylamine. Because the copper microparticles have a surface coated with terpineol and dodecylamine, they have excellent oxidation inhibition in room temperature air and in a humid environment, even though they have a nano-sized particle size of 10 to 100 nm measured by the BET method and a large specific surface area. That is, even when stored in room temperature air, oxidation of the copper microparticles is inhibited, allowing them to be stably stored in room temperature air for long periods of time. Furthermore, because oxidation of the copper microparticles is inhibited even in a humid environment, they can be used in various processes involving moisture.
[0020] Furthermore, the copper microparticles are coated with terpineol and dodecylamine, providing an oxidation-resistant coating layer that inhibits oxidation in room temperature air and in moist environments, thereby inhibiting the formation of copper oxide on the surface of the copper microparticles, including during storage. Furthermore, the sintered copper microparticles have a higher melting point and excellent heat dissipation properties compared to solder and the like. Therefore, copper microparticles can be used for die attach (die bonding), etc., and when used as a bonding material, they can achieve excellent conductivity and heat dissipation while satisfying heat resistance. It is known that in metals, the ratio of thermal conductivity to electrical conductivity is proportional to temperature (Wiedemann-Franz law). Therefore, in copper, which is a metal, increasing electrical conductivity means increasing thermal conductivity. Therefore, in copper microparticles, excellent conductivity means excellent heat dissipation.
[0021] The copper microparticles are surface-coated with terpineol and dodecylamine, but are not dispersed in a solvent or the like, but exist as copper microparticles alone without a solvent or the like. Therefore, when copper microparticles are used, a sintered body can be obtained using only the copper microparticles. From this perspective, copper microparticles are suitable for die attachment (die bonding) and the like. Furthermore, because copper microparticles exist alone, when copper microparticles are used in combination with a solvent, the combination of copper microparticles and solvent is not particularly limited, and the solvent can be selected with great freedom, since the copper microparticles exhibit excellent oxidation inhibition in a humid environment as described above. Furthermore, when copper microparticles are dispersed in a solvent or the like to form a paste, the formation of copper oxide on the surface of the copper microparticles is suppressed even if the paste contains moisture. Therefore, when bonded using the paste, the copper microparticles exhibit conductivity and excellent heat dissipation, making them suitable for die attachment (die bonding) and the like. As described above, the copper microparticles exist as copper microparticles alone without a solvent or the like. That is, the copper microparticles exist as particles alone. The presence of copper microparticles alone also includes a state in which the copper microparticles are dispersed in a gas.
[0022] Here, when dodecylamine is coated on the surface of copper microparticles using a solution, the solution is difficult to handle. Therefore, in order to produce copper microparticles using a simple method, it is preferable to use a small amount of dodecylamine. The surfaces of the copper microparticles are coated with terpineol and dodecylamine, and part of the dodecylamine is replaced with terpineol. Therefore, the amount of dodecylamine used is less than when only dodecylamine is used. Moreover, as described above, copper microparticles whose surfaces are coated with terpineol and dodecylamine have excellent oxidation inhibition properties in the air at room temperature and in a humid environment. A humid environment refers, for example, to water or a solvent containing water.
[0023] [Use of Copper Microparticles] FIG. 1 is a schematic diagram showing an example of a use of copper microparticles of the present invention, and FIG. 2 is a schematic diagram showing another example of a use of copper microparticles of the present invention. Copper microparticles are used, for example, as a bonding material. More specifically, copper microparticles are used as a bonding material to bond a substrate 50 and a power semiconductor element 52 shown in FIG. 1. Copper microparticles are used for die attachment. The copper microparticles form a bonding portion 54 that bonds the substrate 50 and the power semiconductor element 52. The bonding portion 54 is formed by firing the copper microparticles, for example, at a temperature of 200°C for 1 hour in a nitrogen atmosphere. The bonding portion 54 bonds the substrate 50 and the power semiconductor element 52, physically fixing the substrate 50 and the power semiconductor element 52. The copper microparticles can also be used to bond a single substrate 50 and multiple semiconductor elements as shown in FIG. 2. Three semiconductor elements 53a, 53b, and 53c are shown as an example in FIG. 2. The three semiconductor elements 53a, 53b, and 53c are different in size. The three semiconductor elements 53a, 53b, and 53c are bonded to the substrate 50 via a bonding portion 54. Since the three semiconductor elements 53a, 53b, and 53c are different in size, when the bonding material forming the bonding portion 54 is plate-shaped or sheet-shaped, it is necessary to match the size of the bonding material to the sizes of the three semiconductor elements 53a, 53b, and 53c, and it is also necessary to align the positions of the bonding material, which results in poor workability. In contrast, when copper fine particles are used, it is not necessary to match the size of the bonding material to the sizes of the three semiconductor elements 53a, 53b, and 53c, and there is no need to align the positions of the bonding material, and bonding can be performed in a simple manner.
[0024] The sintered copper particles have a higher melting point and higher heat resistance than solder. As a result, even when the ambient temperature exceeds the melting point of solder, the bond between the power semiconductor element 52 and the substrate 50 and the bond between the semiconductor elements 53a, 53b, and 53c and the substrate 50 is maintained, resulting in high durability. In addition, since the sintered copper particles have excellent thermal conductivity, the bonded portions 54 can efficiently conduct heat generated by the power semiconductor element 52 to the substrate 50.
[0025] The substrate 50 is, for example, Si 3 N 4The power semiconductor element 52 is a semiconductor element using a semiconductor such as silicon carbide (SiC), gallium nitride (GaN), gallium oxide, or diamond. The semiconductor elements 53a, 53b, and 53c are semiconductor elements using a general silicon substrate. The semiconductor elements 53a, 53b, and 53c may also be power semiconductor elements. The copper microparticles are not limited to bonding with the power semiconductor element 52 or the semiconductor elements 53a, 53b, and 53c, but can also be used to bond high-frequency devices, light-emitting diodes, semiconductor lasers, and the like. As described above, copper microparticles have excellent thermal conductivity and are suitable for bonding with items that generate a large amount of heat or have a high operating temperature. In addition to the bonding between the power semiconductor element and the substrate and the bonding between the semiconductor element and the substrate, the copper microparticles can also be used for various types of wiring, such as signal wiring and conductive wiring.
[0026] [Method for producing copper microparticles] Next, an example of a method for producing copper microparticles will be described with reference to Fig. 3, but the method for producing copper microparticles of the present invention is not limited to a production method using the copper microparticle production apparatus 10 shown in Fig. 3. Fig. 3 is a schematic diagram showing an example of the copper microparticle production apparatus of the present invention. The copper microparticles described above can be obtained by the copper microparticle production apparatus 10 shown in Fig. 3 (hereinafter simply referred to as the production apparatus 10).
[0027] The manufacturing apparatus 10 includes a plasma torch 12 that generates a thermal plasma flame, a material supply device 14 that supplies raw powder of copper microparticles into the plasma torch 12, a chamber 16 that functions as a cooling tank for generating primary copper microparticles 15, a cyclone 19 that removes coarse particles having a particle size equal to or larger than a specified particle size from the primary copper microparticles 15, and a recovery unit 20 that recovers secondary copper microparticles 18 having a desired particle size classified by the cyclone 19. The chamber 16 and the cyclone 19 are connected by a connecting pipe 21a. The cyclone 19 and the recovery unit 20 are also connected by a connecting pipe 21b that is connected to an inner pipe 19e. The manufacturing apparatus 10 further includes a supply unit 40 that supplies a surface treatment agent to the primary copper microparticles 15 or the secondary copper microparticles 18. The primary copper microparticles 15 and the secondary copper microparticles 18 are both microparticles in the process of being produced as microparticles of the present invention. The copper microparticles of the present invention are obtained by surface-treating the primary copper microparticles 15 or the secondary copper microparticles 18, i.e., the surface-treated copper microparticles 30. The surfaces of the copper microparticles 30 are coated with terpineol and dodecylamine, and for example, have a coating layer (not shown) composed of terpineol and dodecylamine. The material supply device 14, chamber 16, cyclone 19, and recovery section 20 can be, for example, various devices described in JP 2007-138287 A.
[0028] In this embodiment, for example, copper powder is used as a raw material for producing the microparticles. The copper powder has an average particle size appropriately set so that it can easily evaporate in the thermal plasma flame. The average particle size of the copper powder is measured using a laser diffraction method and is, for example, 100 μm or less, preferably 50 μm or less, and more preferably 15 μm or less.
[0029] The plasma torch 12 is composed of a quartz tube 12a and a high-frequency oscillation coil 12b surrounding it. A supply pipe 14a (described later) is provided at the center of the upper portion of the plasma torch 12 for supplying fine particle raw material powder into the plasma torch 12. A plasma gas supply port 12c is formed around the supply pipe 14a (on the same circumference) and has a ring shape. A power supply (not shown) that generates a high-frequency voltage is connected to the high-frequency oscillation coil 12b. When a high-frequency voltage is applied to the high-frequency oscillation coil 12b, a thermal plasma flame 24 is generated. The raw material (not shown) is evaporated by the thermal plasma flame 24, becoming a gaseous mixture. The plasma torch 12 is a processing unit that uses a gas-phase method to turn the raw material into a gaseous mixture.
[0030] The plasma gas supply unit 22 supplies plasma gas into the plasma torch 12. The plasma gas supply unit 22 is connected to the plasma gas supply port 12c via a pipe 22a. Although not shown, the plasma gas supply unit 22 is provided with a supply amount adjustment unit such as a valve for adjusting the supply amount. The plasma gas is supplied from the plasma gas supply unit 22 through the ring-shaped plasma gas supply port 12c into the plasma torch 12 in the directions indicated by arrows P and S.
[0031] The plasma gas used may be, for example, a mixture of hydrogen gas and argon gas. In this case, hydrogen gas and argon gas are stored in the plasma gas supply unit 22. Hydrogen gas and argon gas are supplied from the plasma gas supply unit 22 through the piping 22a and the plasma gas supply port 12c into the plasma torch 12 in the directions indicated by arrows P and S. Argon gas alone may be supplied in the direction indicated by arrow P. Since the plasma gas used may be a gas appropriate for the copper fine particles, such as argon gas, helium gas, hydrogen gas, or nitrogen gas, it is not necessary to use a mixture of gases as the plasma gas, as described above, and a single type of gas may be used as the plasma gas. When a high-frequency voltage is applied to the high-frequency oscillation coil 12b, a thermal plasma flame 24 is generated in the plasma torch 12.
[0032] The temperature of the thermal plasma flame 24 must be higher than the boiling point of the raw material powder. A higher temperature of the thermal plasma flame 24 is preferable because it facilitates the transition of the raw material powder to a gaseous state, but the temperature is not particularly limited. For example, the temperature of the thermal plasma flame 24 can be set to 6000°C, and theoretically it is believed to reach approximately 10000°C. The pressure atmosphere within the plasma torch 12 is preferably below atmospheric pressure. While the pressure of the below-atmospheric pressure atmosphere is not particularly limited, it is, for example, 0.5 to 100 kPa.
[0033] The outside of the quartz tube 12a is surrounded by a concentric tube (not shown), and cooling water is circulated between this tube and the quartz tube 12a to water-cool the quartz tube 12a and prevent the quartz tube 12a from becoming too hot due to the thermal plasma flame 24 generated within the plasma torch 12.
[0034] The material supply device 14 is connected to the upper part of the plasma torch 12 via a supply pipe 14a. The material supply device 14 supplies the raw material into the thermal plasma flame 24 inside the plasma torch 12. The material supply device 14 is not particularly limited as long as it can supply the raw material into the thermal plasma flame 24. For example, the material supply device 14 supplies the raw material into the thermal plasma flame 24 in a particulate dispersed state.
[0035] When the raw material is a powder, for example, the material supply device 14 that supplies copper powder in powder form can be, as described above, for example, the one disclosed in Japanese Patent Application Laid-Open No. 2007-138287. In this case, the material supply device 14 has, for example, a storage tank (not shown) that stores the raw material, a screw feeder (not shown) that transports a fixed amount of the raw material, a dispersing section (not shown) that disperses the raw material transported by the screw feeder into primary particles before it is finally sprayed, and a carrier gas supply source (not shown).
[0036] The raw material is supplied from a carrier gas supply source under extrusion pressure to a thermal plasma flame 24 in the plasma torch 12 via a supply pipe 14a. The material supply device 14 is not particularly limited in configuration as long as it can prevent the raw material from agglomerating and disperse the raw material into the plasma torch 12 while maintaining a dispersed state. An inert gas such as argon gas is used as the carrier gas. The carrier gas flow rate can be controlled using a flow meter such as a float flow meter. The flow rate value of the carrier gas refers to the scale value of the flow meter.
[0037] The chamber 16 is provided adjacent to and below the plasma torch 12, and is connected to a cooling gas supply unit 25 via a pipe 25a. Within the chamber 16, primary copper particles 15, which are fine particles, are generated from the gaseous mixture described above. The chamber 16 also functions as a cooling tank. The cooling gas is also called a quenching gas, and argon gas or the like is used.
[0038] The cooling gas supply unit 25 supplies cooling gas into the chamber 16 via a pipe 25a. The raw material powder is evaporated by the thermal plasma flame 24 to form a gaseous mixture, and the cooling gas supply unit 25 supplies a cooling gas (quenching gas) containing an inert gas to this mixture. The cooling gas (quenching gas) can be, like the plasma gas, argon gas, helium gas, or nitrogen gas. The cooling gas supply unit 25 is connected to the chamber 16 via a pipe 25a. The cooling gas supply unit 25 includes a gas supply source (not shown) in which the cooling gas is stored and a pressure applying means (not shown) that applies extrusion pressure to the cooling gas supplied into the chamber 16. The cooling gas supply unit 25 also includes a pressure control valve (not shown) that controls the amount of gas supplied from the gas supply source. When the cooling gas is argon, for example, argon gas is stored in the gas supply source. The pressure applying means is, for example, a compressor or a blower.
[0039] The cooling gas supply unit 25 supplies argon gas as a cooling gas toward the tail 24b of the thermal plasma flame 24, i.e., the end of the thermal plasma flame 24 opposite the plasma gas supply port 12c, i.e., the terminal end of the thermal plasma flame 24, at an angle of, for example, 45° in the direction of arrow Q, and also supplies the above-mentioned cooling gas from above to below along the inner wall 16a of the chamber 16, i.e., in the direction of arrow R shown in FIG. 1.
[0040] The cooling gas supplied from the cooling gas supply unit 25 into the chamber 16 rapidly cools the gaseous mixture generated by evaporation by the thermal plasma flame 24, thereby obtaining primary fine particles 15. The cooling gas also has additional functions, such as contributing to the classification of the primary fine particles 15 in the cyclone 19. If the primary fine particles 15 collide with each other immediately after generation and form agglomerates, resulting in non-uniform particle sizes, this can lead to a decrease in quality. However, the cooling gas introduced in the direction of arrow Q toward the tail 24b (terminal end) of the thermal plasma flame 24 dilutes the primary fine particles 15, preventing them from colliding with each other and agglomerating. Furthermore, the cooling gas in the direction of arrow R prevents the primary fine particles 15 from adhering to the inner wall 16a of the chamber 16 during the recovery process, thereby improving the yield of the generated primary fine particles 15.
[0041] Although argon gas was used as the cooling gas (quenching gas), the cooling gas (quenching gas) is not limited to argon gas, and nitrogen gas, etc. may also be used. Depending on the manufacturing conditions, the cooling gas (quenching gas) may not be used.
[0042] For example, a gas supply unit 28 that supplies a temperature regulating gas containing an inert gas is provided in the connecting pipe 21a or the connecting pipe 21b. The gas supply unit 28 supplies the temperature regulating gas containing an inert gas to the copper primary particles 15 or the copper secondary particles 18. The gas supply unit 28 has, for example, a valve 28a, and a first gas supply pipe 28b and a second gas supply pipe 28c connected to the valve 28a. The first gas supply pipe 28b is connected to the connecting pipe 21a, and the second gas supply pipe 28c is connected to the connecting pipe 21b. By switching the valve 28a, the temperature regulating gas is supplied to either the first gas supply pipe 28b or the second gas supply pipe 28c, and the temperature regulating gas is supplied into the connecting pipe 21a or the connecting pipe 21b.
[0043] The gas supply unit 28 further includes a pressure applying device (not shown) that applies extrusion pressure to the temperature adjustment gas supplied to the first gas supply pipe 28b or the second gas supply pipe 28c. The pressure applying device is, for example, a compressor or a blower. The gas supply unit 28 also includes a storage unit (not shown) that stores the temperature adjustment gas and a pressure control valve (not shown) that controls the amount of gas supplied. The temperature adjustment gas is, for example, argon gas. The temperature adjustment gas supplied from the gas supply unit 28 to the connecting pipe 21a or the connecting pipe 21b can be used to adjust the gas temperature to a desired level.
[0044] As shown in Fig. 3, the chamber 16 is provided with a cyclone 19 for classifying the copper primary particles 15 into particles of a desired particle size. The cyclone 19 includes an inlet pipe 19a for supplying the primary particles 15 from the chamber 16, a cylindrical outer cylinder 19b connected to the inlet pipe 19a and located at the top of the cyclone 19, a truncated cone section 19c extending downward from the bottom of the outer cylinder 19b and gradually decreasing in diameter, a coarse particle recovery chamber 19d connected to the bottom of the truncated cone section 19c for recovering coarse particles having a particle size equal to or larger than the desired particle size, and an inner pipe 19e protruding from the outer cylinder 19b and connected to a recovery section 20 (described later in detail). The chamber 16 and the inlet pipe 19a are connected by a connecting pipe 21a, and the primary particles 15 move to the cyclone 19 through the connecting pipe 21a. The connecting pipe 21a is a transport path for the primary particles 15.
[0045] An airflow containing primary fine particles 15 is blown from the inlet pipe 19a of the cyclone 19 along the inner peripheral wall of the outer cylinder 19b, and as a result, this airflow flows from the inner peripheral wall of the outer cylinder 19b toward the truncated cone portion 19c as shown by arrow T in Figure 3, forming a downward swirling flow. When the downward swirling flow reverses and becomes an upward flow, the balance between centrifugal force and drag forces prevents coarse particles from joining the upward flow, and they descend along the side surface of the truncated cone portion 19c and are collected in the coarse particle collection chamber 19d. Furthermore, fine particles that are more affected by drag than centrifugal force are discharged out of the cyclone 19 along with the upward flow on the inner wall of the truncated cone portion 19c via the inner pipe 19e and connecting pipe 21b.
[0046] Furthermore, a negative pressure (suction force) is generated from the recovery unit 20, which will be described later in detail, through the inner pipe 19e and the connecting pipe 21b. This negative pressure (suction force) causes the fine particles separated from the swirling airflow to be sucked in as indicated by the symbol U, and is sent to the recovery unit 20 through the inner pipe 19e and the connecting pipe 21b.
[0047] A recovery section 20 for recovering copper microparticles 30 having a desired nanometer-order particle size is provided on the extension of inner tube 19e, which is the outlet of the airflow within cyclone 19. Recovery section 20 includes recovery chamber 20a, filter 20b provided within recovery chamber 20a, and vacuum pump 29 connected via tube 20c provided below recovery chamber 20a. Copper microparticles 30 sent from cyclone 19 are sucked by vacuum pump 29 into recovery chamber 20a, where they are collected and remain on the surface of filter 20b. Note that the number of cyclones used in the above-described manufacturing apparatus 10 is not limited to one, and may be two or more, or no cyclone may be used.
[0048] The supply unit 40 supplies the surface treatment agent St to the copper fine particles downstream of the first gas supply pipe 28b in the connecting pipe 21a or downstream of the second gas supply pipe 28c in the connecting pipe 21b. The surface treatment agent St forms copper fine particles whose surfaces are coated with terpineol and dodecylamine. Here, the chamber 16 side with respect to the connecting pipe 21a is referred to as the upstream side, and the cyclone 19 side is referred to as the downstream side. The supply unit 40 has, for example, a valve 41, and a first supply pipe 41b and a second supply pipe 41c connected to the valve 41. The first supply pipe 41b is connected to the connecting pipe 21a downstream of the first gas supply pipe 28b, and the second supply pipe 41c is connected to the connecting pipe 21b downstream of the second gas supply pipe 28c. The connection position of the first supply pipe 41b on the connecting pipe 21a is referred to as P. 1 The connection position of the second supply pipe 41c on the connection pipe 21b is P 2 The connection position P of the second supply pipe 41c 2 is the connection position P of the first supply pipe 41b 1 It is further downstream than
[0049] The supply unit 40 supplies the surface treatment agent St in a temperature range where the surface treatment agent St does not denature, and to the microparticles (copper primary microparticles 15 or copper secondary microparticles 18) in a state of dispersion in the air before they are collected. More specifically, the supply unit 40 supplies the surface treatment agent St to the copper primary microparticles 15 passing through the connecting pipe 21a or the copper secondary microparticles 18 passing through the connecting pipe 21b. The copper primary microparticles 15 passing through the connecting pipe 21a or the copper secondary microparticles 18 passing through the connecting pipe 21b are microparticles in a state of dispersion in the air before they are collected. The surface treatment agent St is supplied by the supply unit 40 in a temperature range where the surface treatment agent St does not denature, and the surface treatment agent St adheres to the copper primary microparticles 15 or the copper secondary microparticles 18. This surface-treats the copper primary microparticles 15 or the copper secondary microparticles 18, forming copper microparticles 30 whose surfaces are coated with terpineol and dodecylamine. The coating of terpineol and dodecylamine also prevents fusion between the copper particles 30. The surface condition of the surface-treated copper particles 30 can be examined using, for example, an FT-IR (Fourier transform infrared spectrophotometer).
[0050] The method for supplying the surface treatment agent St by the supply unit 40 is not particularly limited, and an example is a method in which the surface treatment agent St is formed into droplets and sprayed onto the copper secondary microparticles 18. As described above, the surface treatment agent St is supplied in a temperature range in which the surface treatment agent St does not denature. Specifically, the temperature range in which the surface treatment agent St does not denature is a temperature range in which terpineol and dodecylamine do not denature. The temperature range in which the surface treatment agent St does not denature is a temperature range determined based on the temperature measured by simultaneous differential thermal analysis and thermogravimetry (TG-DTA). The temperature range in which the surface treatment agent St does not denature is a temperature range in which the weight loss rate of the surface treatment agent St in simultaneous differential thermal analysis and thermogravimetry is 50% by mass or less. The weight loss rate is more preferably 30% by mass or less, and even more preferably 10% by mass or less. For the simultaneous differential thermal analysis and thermogravimetry, a STA7200 (product name) from Hitachi High-Tech Science Corporation is used.
[0051] The surface treatment agent St uses terpineol and dodecylamine to coat the copper fine particles (fine particle bodies (not shown)). The surface treatment agent St may contain an organic solvent. As the surface treatment agent St, a solution of terpineol and dodecylamine is sprayed onto the copper primary fine particles 15 or the copper secondary fine particles 18 using a spray gas. The spray gas is, for example, argon gas.
[0052] In the method for producing copper microparticles, the amount of terpineol introduced per unit area is 1.36 × 10 -3 g / m 2 The amount of terpineol introduced per unit area is preferably 1.36 × 10 or more. -3 g / m 2 In the method for producing copper microparticles, the amount of dodecylamine introduced per unit area is 1.20 × 10 -4 g / m 2 Furthermore, it is preferable that the amount of dodecylamine introduced per unit area is 3.55×10 or more. -3 g / m 2In the method for producing copper microparticles, the amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is 1.48 × 10 or less. -3 g / m 2 The total amount of terpineol and dodecylamine introduced per unit area is preferably 1.48 × 10 or more. -3 g / m 2 If the amount is above this, the copper microparticles can fully exhibit oxidation resistance to the atmosphere at room temperature and oxidation resistance to moisture. As mentioned above, dodecylamine solutions are difficult to handle, and terpineol is easier to handle than dodecylamine. In the method for producing copper microparticles, part of the dodecylamine is replaced with terpineol. Therefore, the amount of dodecylamine used is less than when only dodecylamine is used. This makes it easier to handle the surface treatment agent, and copper microparticles can be produced by a simple method. Thus, from the viewpoint of handling, it is sufficient to replace part of the dodecylamine with terpineol, and it is preferable that the amount of dodecylamine is small enough to allow the produced copper microparticles to exhibit sufficient oxidation resistance to the atmosphere and moisture at room temperature. The amount of dodecylamine is 1.20 x 10 -4 g / m 2 It is preferable that this is equal to or greater than this.
[0053] (Organic solvent) The organic solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the organic solvent include alcohols such as ethanol and methanol, ketones such as acetone, alkyl halides, amides such as formamide, sulfoxides such as dimethyl sulfoxide, heterocyclic compounds, hydrocarbons, esters such as ethyl acetate, and ethers. These may be used alone or in combination of two or more.
[0054] The manufacturing apparatus 10 may have a sensor (not shown) that measures the temperature of the transport path of the copper primary particles 15 or the copper secondary particles 18. The temperature measurement result of this sensor is used to determine whether or not the temperature range is within which the surface treatment agent St will not denature. In this case, the temperature measurement result is output to, for example, the supply unit 40. The supply unit 40 can determine whether or not the temperature range is within which the surface treatment agent St will not denature based on the temperature measurement result of the transport path of the copper primary particles 15 or the temperature measurement result of the transport path of the copper secondary particles 18 by the sensor. If the temperature of the transport path of the copper primary particles 15 or the copper secondary particles 18 is within the temperature range within which the surface treatment agent St will denature, for example, the flow rate of the temperature adjustment gas supplied from the gas supply unit 28 is changed. As described above, the temperature measurement result of the sensor is used to determine whether or not the temperature range is within which the surface treatment agent St will not denature. 1 It is preferable to provide the sensor upstream of the connecting pipe 21a. For this reason, the sensor is provided, for example, in the connecting pipe 21a. The configuration of the sensor is not particularly limited as long as it can measure temperature, but it is preferable that the measurement time be short. For this reason, for example, a resistance thermometer, a radiation thermometer, an infrared radiation temperature sensor, a thermistor, etc. can be used as the sensor.
[0055] Next, an example of a method for producing copper microparticles using the above-described production apparatus 10 will be described. First, copper powder having an average particle size of 15 μm or less is fed into the material supply device 14 as raw powder for the copper microparticles. Using argon gas and hydrogen gas, for example, as the plasma gas, a high-frequency voltage is applied to the high-frequency oscillation coil 12b to generate a thermal plasma flame 24 in the plasma torch 12. Next, the copper powder is gas-transported using argon gas, for example, as the carrier gas, and supplied into the thermal plasma flame 24 in the plasma torch 12 via the supply pipe 14a. The supplied copper powder evaporates in the thermal plasma flame 24 to form a gaseous mixture, and primary copper microparticles 15 are generated from the gaseous mixture in the chamber 16 without using a cooling gas.
[0056] The primary copper particles 15 obtained in the chamber 16 then pass through the connecting pipe 21a and are blown into the inlet pipe 19a of the cyclone 19 along the inner circumferential wall of the outer cylinder 19b, along with the airflow. As a result, the airflow flows along the inner circumferential wall of the outer cylinder 19b, forming a swirling flow and descending, as indicated by arrow T in FIG. 3 . When the descending swirling flow reverses and becomes an ascending flow, the balance between centrifugal force and drag forces prevents coarse particles from joining the ascending flow, causing them to descend along the side of the truncated cone portion 19c and be collected in the coarse particle collection chamber 19d. Furthermore, particles affected more by drag than centrifugal force are discharged from the inner wall of the truncated cone portion 19c along with the ascending flow and out of the cyclone 19. The discharged secondary copper particles 18 are sucked in the direction indicated by symbol U in FIG. 3 by the negative pressure (suction force) from the collection section 20 generated by the vacuum pump 29, passing through the inner pipe 19e and the connecting pipe 21b.
[0057] When the copper primary particles 15 pass through the connecting pipe 21a or the copper secondary particles 18 pass through the connecting pipe 21b, a temperature-adjusting gas is supplied from the gas supply unit 28 through the first gas supply pipe 28b into the connecting pipe 21a to cool the copper primary particles 15, or through the second gas supply pipe 28c into the connecting pipe 21b to cool the copper secondary particles 18. After the temperature-adjusting gas adjusts the copper primary particles 15 or the copper secondary particles 18 to a temperature range where the surface treatment agent St does not denature, the surface treatment agent St is further supplied from the supply unit 40 into the connecting pipe 21a in the form of, for example, a spray to the copper primary particles 15, thereby surface-treating the copper primary particles 15. Furthermore, the surface treatment agent St is supplied from the supply unit 40 into the connecting pipe 21b in the form of, for example, a spray to the copper secondary particles 18, thereby surface-treating the copper secondary particles 18. The surface-treated primary copper particles 15 or secondary copper particles 18, i.e., copper particles 30, are sent to the recovery section 20, and the copper particles 30 are recovered by the filter 20b of the recovery section 20. In this manner, the copper particles 30 are obtained.
[0058] When the copper microparticles 30 are collected in the collection section 20, the internal pressure in the cyclone 19 is preferably equal to or lower than atmospheric pressure. The particle size of the copper microparticles 30 is specified to any particle size on the order of nanometers depending on the purpose. While the present invention uses a thermal plasma flame as a heat source to form the primary copper microparticles, other gas phase methods can also be used to form the primary copper microparticles. Therefore, the gas phase method is not limited to using a thermal plasma flame, and may be, for example, a flame method for forming the primary copper microparticles. The method for producing primary microparticles using a thermal plasma flame is called a thermal plasma method.
[0059] Here, the flame method is a method of synthesizing fine particles by passing a copper-containing raw material through a flame using a flame as a heat source. In the flame method, the copper-containing raw material is supplied to the flame, and copper fine particles are generated in the flame to obtain primary copper fine particles 15. Furthermore, a surface treatment agent St is supplied to the primary copper fine particles 15 or the secondary copper fine particles 18 to produce copper fine particles. Note that the same surface treatment agent as that used in the thermal plasma method can also be used in the flame method.
[0060] The present invention is basically configured as described above. While the copper microparticles and the method for producing copper microparticles of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0061] The copper microparticles of the present invention will be described in more detail below. In the examples, copper microparticles of Examples 1 and 2 and copper microparticles of Comparative Examples 1 to 3 were produced. The copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Examples 1 to 3 were produced using a production apparatus 10 shown in Figure 3. The production conditions are shown below.
[0062] Example 1 In Example 1, copper powder with an average particle size of 5 μm was used as the raw material powder. The average particle size of the copper powder was measured using a particle size distribution analyzer. The particle size distribution analyzer used was an MT3300 (product name) manufactured by Microtrac Bell Co., Ltd. The production conditions for the copper microparticles were a constant plasma input of 13 kW and a fixed pressure inside the plasma torch of 40 kPa. Argon gas was used as the carrier gas. The flow rate of the argon gas was 5 liters / minute (standard state equivalent). Argon gas and hydrogen gas were used as the plasma gas. The flow rate of the argon gas was 200 liters / minute (standard state equivalent), and the flow rate of the hydrogen gas was 5 liters / minute (standard state equivalent). Argon gas was used as the quenching gas. The flow rate of the argon gas was 600 liters / minute (standard state equivalent).
[0063] In Example 1, the surface treatment agent was terpineol (C 10 H 18 Ethanol was used as the solvent, and a solution containing terpineol and dodecylamine (terpineol concentration: 20 W / W%, dodecylamine concentration: 3 W / W%) was sprayed onto the copper secondary particles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. The amount of terpineol introduced was 6.5 W / W% relative to the amount of copper raw material powder supplied, and the amount of dodecylamine introduced was 1.0 W / W% relative to the amount of copper raw material powder supplied. The mass ratio of terpineol to dodecylamine was 87:13. Terpineol manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. was used. Dodecylamine manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. was used. Ethanol manufactured by Junsei Chemical Co., Ltd. (product code: 17065-1283) was used.
[0064] Example 2 Example 2 is similar to Example 1, except that the mass ratio of terpineol to dodecylamine in the surface treatment agent was changed to 96:4. In Example 2, the amount of terpineol introduced was 7.8 W / W % relative to the amount of copper raw material powder supplied, and the amount of dodecylamine introduced was 0.36 W / W % relative to the amount of copper raw material powder supplied. The amounts introduced per unit area shown in Table 1 below were calculated by multiplying the minimum weight loss rate up to a temperature of 500°C, determined in a nitrogen atmosphere using simultaneous differential thermal-thermogravimetry (TG-DTA), by the specific surface area ("BET (m)" in Table 1 below) measured based on the BET method. 2 In Examples 1 and 2, the amounts of terpineol and dodecylamine introduced per unit area shown in Table 1 below are values calculated by allocating the previously determined amounts introduced per unit area based on the mass ratio of terpineol to dodecylamine.
[0065] Comparative Example 1 Comparative Example 1 was similar to Example 1, except that, unlike Example 1, only terpineol was used as the surface treatment agent. In Comparative Example 1, ethanol was used as the solvent, and a solution containing terpineol (terpineol concentration: 23 W / W%) was sprayed onto the copper secondary fine particles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. Comparative Example 2 Comparative Example 2 was similar to Example 1, except that, unlike Example 1, only terpineol was used as the surface treatment agent, and the flow rate of the quenched argon gas was set to 250 liters / minute (standard state equivalent). In Comparative Example 2, ethanol was used as the solvent, and a solution containing terpineol (terpineol concentration: 17 W / W%) was sprayed onto the copper secondary fine particles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. In Comparative Examples 1 and 2, terpineol manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. Ethanol manufactured by Junsei Chemical Co., Ltd. (product code 17065-1283) was used.
[0066] Comparative Example 3 Comparative Example 3 was similar to Example 1, except that, unlike Example 1, only dodecylamine was used as the surface treatment agent. In Comparative Example 3, ethanol was used as the solvent, and a solution containing dodecylamine (dodecylamine concentration: 23 W / W%) was sprayed onto the copper secondary microparticles 18 (see FIG. 3) from the second supply pipe 41c (see FIG. 3) using a spray gas. Argon gas was used as the spray gas. Dodecylamine manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. Ethanol manufactured by Junsei Chemical Co., Ltd. (product code 17065-1283) was used. In Comparative Examples 1 to 3, the amounts of terpineol and dodecylamine introduced per unit area shown in Table 1 below were calculated by allocating the previously determined amounts introduced per unit area based on the mass ratio of terpineol to dodecylamine. Comparative Examples 1 and 2 used only terpineol, and the amount of dodecylamine introduced per unit area was "0 (zero)." In Comparative Example 3, only dodecylamine was used, and the amount of terpineol introduced per unit area was "0 (zero)."
[0067] The particle size was measured by the BET method for the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Examples 1 to 3. Macsorb HM-1208 (trade name) manufactured by Mountech Co., Ltd. was used to measure the particle size of the copper microparticles.
[0068] For the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Examples 1 to 3, the minimum weight loss rate up to a temperature of 500°C in a nitrogen atmosphere was determined. It is believed that heating up to 500°C would cause much of the organic matter present on the copper particle surface to thermally decompose and disappear. Therefore, the minimum weight loss rate determined by heating up to 500°C is considered to be the introduction rate of the particle surface coating. Therefore, the minimum weight loss rate up to a temperature of 500°C in a nitrogen atmosphere divided by the BET value is the introduction amount per unit area in Table 1 below. The minimum weight loss rate up to a temperature of 500°C in the nitrogen atmosphere was determined by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) of the copper microparticles. A STA7200 (trade name) manufactured by Hitachi High-Tech Science Corporation was used for the differential thermal analysis and thermogravimetry analysis. The nitrogen atmosphere refers to an atmosphere in which nitrogen gas with a purity of 99.99 (99.99% by volume of nitrogen) is constantly flowing and in which the oxygen concentration is 3 ppm by volume or less. Therefore, the nitrogen atmosphere can have an oxygen concentration of 3 ppm by volume or less, and the nitrogen may be mixed with a gas that does not react with copper, such as a rare gas, or its decomposition products. The oxygen concentration can be measured, for example, using a low-concentration oxygen analyzer PS-820-L (product name) manufactured by Iijima Electronics Co., Ltd.
[0069] The oxidation resistance of the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Examples 1 to 3 was evaluated. The oxidation resistance was evaluated in a room temperature atmospheric environment and in an aqueous environment. To evaluate the oxidation resistance in a room temperature atmospheric environment, the prepared copper microparticles were first placed in a glass container in the atmosphere and sealed, and the glass container was maintained at room temperature (25°C). The atmosphere inside the glass container was also an atmospheric environment. Every week, crystal structure analysis was performed on the copper microparticles in the glass container using X-ray diffraction to confirm the presence or absence of oxidation of the copper microparticles. The atmospheric composition of the above-mentioned atmospheric atmosphere was as described above. The atmospheric composition, i.e., the air composition, was 78.08 vol% nitrogen, 20.95 vol% oxygen, 0.93 vol% argon, and 0.03 vol% carbon dioxide. In the evaluation of oxidation resistance in a room temperature atmospheric environment, if a copper oxide peak was obtained in crystal structure analysis using X-ray diffraction, the copper microparticles were considered to be oxidized. Those in which oxidation of copper particles was confirmed within two weeks were rated "C", those in which oxidation of copper particles was confirmed between two and three weeks were rated "B", and those in which oxidation of copper particles was not confirmed even after three weeks were rated "A".
[0070] Among the evaluations of oxidation resistance, the evaluation of oxidation resistance in an aqueous environment involved first immersing the prepared copper microparticles in water and subjecting them to ultrasonic dispersion treatment for 1 minute. The copper microparticles were then naturally dried, and the resulting dry powder was subjected to crystal structure analysis using X-ray diffraction to confirm the presence or absence of oxidation of the copper microparticles. In the evaluation of oxidation resistance in an aqueous environment, if a copper oxide peak was obtained in the crystal structure analysis using X-ray diffraction, the copper microparticles were deemed to have oxidized. The evaluation of oxidation resistance in an aqueous environment was based on the following evaluation criteria. Evaluation criteria: A: No copper oxide peak was obtained (oxidation of the copper microparticles could not be confirmed). B: A small copper oxide peak was obtained. C: A copper oxide peak was obtained (oxidation of the copper microparticles could be confirmed). Note that the small copper oxide peak in evaluation B above refers to a ratio a / b of 0.2 or less, where a is the maximum value a of the copper oxide peaks at 35 to 40 degrees observed in crystal structure analysis using X-ray diffraction, and b is the maximum value b of the copper peaks at 40 to 45 degrees. The copper oxide peak in the above-mentioned evaluation C refers to a sample in which the ratio a / b exceeds 0.2. Furthermore, the absence of a copper oxide peak in the above-mentioned evaluation A refers to a sample in which a copper oxide peak is not observed in crystal structure analysis by X-ray diffraction. The above-mentioned evaluation A refers to a sample in which the ratio a / b is 0.03 or less.
[0071] The copper microparticles of Examples 1 and 2 and Comparative Examples 1 to 3 were evaluated for handleability. Handling is an index for evaluating the ease of manufacturing copper microparticles. When the amount of dodecylamine introduced is large, the handleability of the solution used in the surface treatment agent becomes poor. For this reason, among the copper microparticles of Examples 1 and 2 and the copper microparticles of Comparative Examples 1 to 3, Comparative Example 3, which contained only dodecylamine, had poor solution handleability and was rated "C." In Examples 1 and 2, the amount of dodecylamine introduced was small, which did not affect solution handleability and was rated "A." In Comparative Examples 1 and 2, dodecylamine was not used, and terpineol had good solution handleability and was rated "A."
[0072]
[0073] As shown in Table 1, the copper microparticles of Examples 1 and 2, even though terpineol was used for the surface coating, had better oxidation resistance in an ambient environment at room temperature and in an aqueous environment, and also had better handleability than Comparative Examples 1 to 3. Comparative Examples 1 and 2 used only terpineol and had poor oxidation resistance in water. Comparative Example 3 used only dodecylamine and had poor handleability. In Example 1, the amount of terpineol introduced per unit area was 1.36 × 10 -3 g / m 2 When the oxidation resistance of the copper particles is less than 100%, the oxidation resistance of the copper particles in the above-mentioned room temperature atmospheric environment is evaluated as "B", and the other evaluations are the same as those in Example 1.
[0074] DESCRIPTION OF SYMBOLS 10 Copper microparticle manufacturing apparatus (manufacturing apparatus) 12 Plasma torch 12a Quartz tube 12b High frequency oscillation coil 12c Plasma gas supply port 14 Material supply device 14a Supply pipe 15 Primary microparticles 16 Chamber 18 Secondary microparticles 19 Cyclone 19a Inlet pipe 19b Outer cylinder 19c Circular truncated cone portion 19d Coarse particle recovery chamber 19e Inner pipe 20 Recovery section 20a Recovery chamber 20b Filter 21a, 21b Connecting pipe 22 Plasma gas supply section 22a Piping 24 Thermal plasma flame 25 Cooling gas supply section 25a Piping 28 Gas supply section 28a Valve 28b First gas supply pipe 28c Second gas supply pipe 29 Vacuum pump 30 Copper microparticles 40 Supply section 41 Valve 41b First supply pipe 41c Second supply pipe 50 Substrate 52 Power semiconductor element 53a, 53b, 53c Semiconductor element 54 Joint St Surface treatment agent
Claims
1. Copper particles having a surface coated with terpineol and dodecylamine and a particle size of 10 to 100 nm as measured by the BET method.
2. The amount of terpineol introduced per unit area is 1.36 x 10 -3 g / m 2 The copper fine particles according to claim 1 .
3. The amount of dodecylamine introduced per unit area is 1.20 x 10 -4 g / m 2 The copper fine particles according to claim 1 .
4. The amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is 1.48 × 10 -3 g / m 2 The copper fine particles according to claim 2 .
5. A method for producing copper microparticles, comprising the steps of: supplying a carrier gas in which copper powder is dispersed into a thermal plasma flame, and then supplying a cooling gas to an end of the thermal plasma flame to produce microparticles; and supplying a surface treatment agent containing terpineol and dodecylamine to the microparticles in a temperature range in which the surface treatment agent is not denatured, and to the microparticles in an air-dispersed state before the microparticles are recovered.
6. The amount of terpineol introduced per unit area is 1.36 x 10 -3 g / m 2 The method for producing copper microparticles according to claim 5 .
7. The amount of dodecylamine introduced per unit area is 1.20 x 10 -4 g / m 2 The method for producing copper microparticles according to claim 5 .
8. The amount of terpineol introduced per unit area is greater than the amount of dodecylamine introduced per unit area, and the total amount of terpineol and dodecylamine introduced per unit area is 1.48 × 10 -3 g / m 2 The method for producing copper microparticles according to claim 6, wherein 9. A method for producing copper microparticles according to any one of claims 5 to 8, wherein the cooling gas is argon gas, helium gas or nitrogen gas.
10. A method for producing copper microparticles described in any one of claims 5 to 8, wherein the plasma gas of the thermal plasma flame is argon gas, helium gas, hydrogen gas or nitrogen gas.
Citation Information
Patent Citations
Method for producing copper particulate dispersion
JP2010174312A
Method for producing copper fine particle, copper fine particle, paste composition, semiconductor device and electric / electronic component
JP2017206755A
Conductive metal paste and its manufacturing method
JP4155821B2