Electrically anisotropic antifouling coatings
Electrically anisotropic self-polishing coatings using conductive polyaniline and graphene oxide nanocomposites address the inefficiencies of current antifouling technologies by preventing biofilm formation and offering flexible foul-release mechanisms, achieving long-lasting protection and reduced maintenance costs for marine surfaces.
Patent Information
- Application Number
- PCT/GR2023/000025
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-05-29
- Publication Date
- 2024-10-31
AI Technical Summary
Current antifouling coatings for marine surfaces are ineffective in both static and dynamic conditions, have environmental toxicity concerns, and high maintenance costs, failing to provide long-lasting protection against biofouling without releasing volatile organic compounds or using biocides, and require costly priming and multiple coating layers.
Development of electrically anisotropic, self-polishing coatings using conductive polyaniline nanorods decorated with magnetite nanoparticles and graphene oxide sheets modified with titanium dioxide, combined with a high molecular weight water-soluble resin, which creates a synergistic antimicrobial and photocatalytic effect that prevents biofilm formation and enhances charge dissipation, allowing for flexible nanorod exposure and foul-release mechanisms.
The coating provides sustained anti-fouling performance for up to 6 weeks in static conditions and low hydrodynamic resistance in dynamic conditions, reducing maintenance costs and fuel consumption, while being environmentally friendly and applicable without prior surface priming, with enhanced corrosion resistance and extended functionality.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] DESCRIPTION
[0002] ELECTRICALLY ANISOTROPIC ANTIFOULING COATINGS.
[0003] FIELD OF THE INVENTION
[0004] The present invention refers to a new method of developing electrically conductive and electrically anisotropic coatings with high anti-fouling performance and prolonged functionality for solid surfaces. The method describes the formulation of the coating solution and its application to substrates which come in contact with water, e.g., ship hulls to combat biofouling.
[0005] BACKGROUND OF THE INVENTION
[0006] Biofouling is the accumulation of living organisms, i.e., microorganisms, algae, plants and small animals on solid surfaces. It is manifested by the development of biofilms, which adhere strongly to the substrate and are often difficult to remove because they are highly resistant to biocides and antibiotics.
[0007] Biofouling degrades the intended function of the objects to which these organisms have access. In the maritime sector, for example, it poses significant technical, scientific and economic challenges. In the marine environment, any surface in contact with seawater is subject to biological pollution. Through natural adsorption and within a few minutes, it is colonized by proteins and organic matter, which act as seeds for the development of biofilms. The latter are rapidly formed (e.g., within 48 hours), thus gradually causing macrofouling (secondary and tertiary colonization), i.e., the attachment of marine organisms such as algae and barnacles to the hull of a ship, which reduces its speed and maneuverability and significantly increases its fuel consumption. Hard deposits, in particular, may lead to power losses of more than 85%.
[0008] This natural phenomenon is a huge economic problem for the shipping industry, because it increases the costs associated with the maintenance and repair of vessels, as dry docking for cleaning becomes more often necessary. At the same time, there are also undesirable ecological impacts, such as when a vessel with biological pollution is moved between ports, as non-native species are inadvertently transferred from one area to another.
[0009] It should be noted that biofouling of a ship's reefs causes an increase in their roughness, which to some extent is also due to physical factors such as mechanical detachments, structural defects, hydrodynamic resistance of paints, etc. It has been calculated that for every 10-20 pm increase in reef roughness, the frictional resistance at high speeds increases by 0,5%. To date, numerous attempts aiming to develop anti-fouling coatings have been reported, based on the recent developments in biology, physics and chemistry.
[0010] Biological methods involve the use of enzymes or metabolites secreted by cells as substitutes for traditional biocides. The organic secretions inhibit the growth of their competitors and are biodegradable. This approach has limited success because such substances rather repel, than kill microorganisms. Also, some technical difficulties, such as the design of the coating matrix or balancing the effectiveness and lifetime of the coating, remain. In addition, it is difficult to predict the impact of metabolites and enzymes on the marine environment if these are widely used in reef paints. Among the natural methods, seawater electrolysis is perhaps the most common. Here the coating acts as an anode, producing hypochlorous acid (HC1O), ozone bubbles, hydrogen peroxide or even bromine. Due to their oxidizing capacity, these compounds spread through the hull of the ship and eliminate the pollution. However, due to the high surface tension drop, the corrosion of the steel is intensified and the effectiveness of the method is limited to small vessels (tugs, ferries and cargo vessels) and water circulation pipelines.
[0011] Traditionally, chemical biocides have been considered the standard approach to control marine biological pollution. Compounds such as tributyltin oxide (C24Hs4OSn2) and tributyltin fluoride (CnH^FSn) were incorporated into polymeric matrices to produce antifouling paints. Due to their low harshness and the duration of their antifouling activity (3-5 years), self-polishing copolymer antifouling paints containing tributyltin (TBT) dominated the market and in 1998 were used in over 70% of the world's merchant fleet, which was estimated to have generated savings of $5,7 billion to the world shipping industry. However, in 2008 the International Maritime Organization (IMO) declared the use of TBT toxic to the marine environment, so in the following period the research for the formulation of effective and environmentally safe reef paints that would not contain TBT but another biocide or would be biocide-free, was intensified. Today, due to the lack of effective alternatives, antifouling paints containing biocides, e.g., based on copper and its compounds, which are considered as a transitional stage between toxic and non-toxic coatings, dominate the antifouling coating market. Copper oxide is recommended by Environmental Protection Agencies (EP A) as a replacement for TBT, since in water it can bind to other substances; therefore, its toxicity is reduced. In many antifouling paints, copper is also combined with herbicides, as it has been observed that during the initial stages of colonization of any submerged object in the sea, bacteria and single-celled phytoplanktonic organisms attach to it, which can be significantly reduced by the addition of biocide enhancers. Thus, the multicellular organisms that follow are unable to attach themselves to the submerged solid object.
[0012] In general, however, it should be noted that none of the formulations that replaced the TBT-containing antifouling paints were as effective, long- lasting and low-priced. Moreover, some biocides that enhance the action of copper are shown to have collateral environmental damage and are also banned. Materials for marine applications must comply with new stricter rules regarding the protection of the environment, aquatic organisms and human health. Therefore, modem antifouling coatings are turning to solutions that do not rely on the use of biocides and do not release volatile organic compounds (VOCs) into the environment.
[0013] Furthermore, it is generally accepted that, apart from the low toxicity that its active ingredient must exhibit, the efficacy and cost of an antifouling coating are the most important factors for its widespread application. With regards to anti-fouling efficacy, it should be noted that this is a necessary requirement under both static and dynamic conditions. Unfortunately, current antifouling paints do not perform sufficiently in static conditions. A typical modem silicone antifouling paint initiates the foul-release activity of reefs at speeds of at least 15-20 knots. Micro-organisms such as diatoms create a highly adhesive film that is difficult to remove. Existing antifouling paints are not effective when the ship is at anchor, with the majority of them being functional for 30-40 days at the most. Continuing, seawater properties such as salinity and turbidity, as well as temperature and pH fluctuations have a significant effect on the ability of microorganisms, algae and plants to attach to a surface. For example, variations in pH affect the solubility of biocides and the rate of coating erosion. Annual variations and seasonal temperature changes have a significant effect on the reproductive cycles of micro-organisms and, consequently, on the types of micro-organisms growing, the rate of coating erosion and the extent of biofouling. Therefore, an effective anti-fouling coating should be fully functional over a wide range of conditions. Furthermore, as far the cost of the antifouling paint is concerned, in addition to the cost of application, the cost of removal should be taken into account. The cost of priming the surface should also not be overlooked. Similarly, in order to assess economic viability and potential economies of scale, the facility of the application method as well as the drying time or the number of coating layers required until the paint reaches a critical functional thickness should not be overlooked.
[0014] The above conditions are not met by the majority of modem antifouling paints. It is therefore necessary to develop new, sustainable coatings with high anti-fouling performance and low hydrodynamic resistance for the hulls of ships, boats and high-speed crafts. It is an object of the present invention to provide a method of developing an antifouling paint that satisfies one or more of the above requirements.
[0015] It should also be noted that biofouling does not only affect the hulls of ships, as it occurs on a wide range of surfaces of components, systems or structures, such as, for example, water circulation pipes, heating cooling systems and medical devices. In the medical sector, for example, non- selective adsorption of proteins often leads to failure of medical devices and equipment, while frequent contact of hospital equipment with water leads to bacterial contamination, which poses risks to staff and patients.
[0016] Consequently, there is a need for an antifouling material capable of effectively preventing the formation of biofilms and / or an antifouling technology for the surface treatment of a solid in contact with water or moisture.
[0017] To date, and regardless of the surface, the basic approach to prevent biofouling has been based on preventing bacterial adhesion and biofilm formation through the development of anti-stick and anti-microbial coatings. The latter are prepared by incorporating antimicrobial agents into fouling-repellent materials through covalent bonding, layer-by-layer deposition or composite structures, e.g., core-shell structures. The resulting structures may combine biocide substrates and antifouling topcoats, contact-active antimicrobial topcoats and antifouling substrates, or uniformly mixed antimicrobial and antifouling components in an appropriate layering. The aim is to achieve, as far as possible, simultaneous active and passive antibacterial or antimicrobial function.
[0018] For the development of effective anti-fouling protection, different materials and synthetic routes have been reported. The biocides used can be organic (e.g., tralopyril), organometallic (e.g., zinc pyrithione) or inorganic (e.g., metallic copper or copper oxide) and are dispersed either in water-soluble or non-water-soluble matrices of natural / synthetic resins and polymers. Antifouling behavior may also be manifested without the use of biocides, e.g., through the use of amphoteric silanes and copolymers, nitric oxide, sulphonic acid salts, carbon allotropes, antimicrobial peptides, modified polysaccharides, etc.
[0019] U.S. Pat. 2022 / 11,427,714 B2 refers to multilayer antifouling coatings, consisting of an algicidal primer, a hydrophobic polymer intermediate and a metallic silver-copper mixture as the top layer, for heating and cooling systems.
[0020] U.S. Pat. 2022 / 11,472,967 Bl describes a mixture of resins containing biocides.
[0021] U.S. Pat. 2022 / 0049112 Al refers to antifouling coatings of a copolymer blend for various surfaces. WO 2021 / 191388 Al describes anti-fouling coatings using resins and polymers containing organic biocides in core-shell structures.
[0022] WO 2022 / 261559 A2 describes hydrophilic biofouling release coatings based on amphoteric silanes.
[0023] EP 3 831 898 Al discloses the direct application of an antifouling composition based on a triisopropylsilyl methacrylate copolymer directly on aged antifouling coatings, without their prior removal.
[0024] WO 2016 / 187698 Al discloses a chemical composition based on polymeric resins of catechol derivatives and hydrophilic polymers for limiting biofouling and protein binding in medical devices.
[0025] U.S. Pat. 2020 / 0231822 Al describes mixtures of carbon allotropes that prevent biofouling on conductive surfaces, e.g., on electrodes, in molecular diagnostics applications.
[0026] U.S. Pat. 2022 / 0332955 Al discloses environmentally friendly antifouling paints based on sulfonic acid salts.
[0027] U.S. Pat. 2022 / 11,518,891 B2 discloses self-polishing antifouling paints based on water-soluble polyurethane crosslinked with acrylic acid-modified polysaccharides.
[0028] WO 2022 / 251963 Al discloses anti-fouling coatings for medical devices and implants based on a combination of polymeric resins (e.g., dopamine), high molecular weight hydrophilic polymers and conjugated antimicrobial peptides.
[0029] WO 2022 / 173816 Al refers to superhydrophobic coatings containing zinc oxide, copper and perfluoroalkylsiloxane for preventing biofilm growth on any surface.
[0030] WO 2019 / 079765 Al describes coatings, which are cured by UV irradiation, for biomedical applications. Their action is based on the combination of, killing bacteria through the release of nitric oxide from doped polymers, and repelling proteins through covalently bonded amphoteric polymers as a top coat. The coated articles exhibit anti-fouling, anti-microbial and / or anti-thrombotic properties.
[0031] U.S. Pat. 2021 / 0301153 Al discloses high strength, water-based antifouling coatings for ships, based on synthetic resins and a combination of biocides.
[0032] Pat. WO 2021 / 226699 A9 describes hydrophobic coatings of high mechanical strength, based on epoxy resins, for simultaneously achieving anti-fouling and anti-corrosion protection on various surfaces exposed to water and moisture.
[0033] Besides deterrent mechanisms of biofilm formation, the operating principle of an anti-fouling coating may also be based on physical factors, such as the free oscillation of flexible fibers which releases biofouling under buoyant conditions. For example, U.S. Pat. 2012 / 8,278,226 B2 relates to antifouling coatings based on polyamide fibers embedded in a matrix of waterproof polyurethane through the electrostatic flocking technique. The coatings are suitable for marine equipment surfaces in order to release biofouling due to the free oscillation of the polyamide fibers under dynamic conditions.
[0034] In line with the above, there is a clear need to develop more effective technologies and environmentally friendly anti-fouling materials, whose operating principle would allow their application on various substrates with different requirements.
[0035] It is an object of the present invention to develop an anti -fouling coating for the hulls of ships and vessels, which will be effective in both static and dynamic conditions.
[0036] It is also an object of the present invention to develop an anti -fouling coating for surfaces in contact with water or moisture, which will have a broad applicability.
[0037] DETAILED DESCRIPTION OF THE INVENTION
[0038] The present invention describes a method of developing durable selfpolishing anti-biofouling coatings for solid surfaces in contact with water. The preparation of the coatings includes environmentally friendly antimicrobial and conductive, electrically anisotropic nanostructures in combination with a high molecular weight water-soluble resin.
[0039] The object of the present invention is therefore the development of antifouling coatings mainly for the protection of ship reefs, without, however, excluding their application by conventional techniques to other surfaces which are in contact with water and moisture and therefore subject to biofouling. The protection provided by the coating is based on the synergistic action of conductive antimicrobial nanocomposites with electrical anisotropy, namely conductive polyaniline (PANI) nanorods externally decorated with magnetite (FesCfi) nanoparticles, which are oriented out-of-the plane defined by graphene oxide (GO) sheets modified with titanium dioxide (TiO2) nanoparticles.
[0040] The coating solution is a water-soluble dispersion. The polyaniline used is an attractive material, as it has a low price, a facile synthesis procedure, high thermal stability and satisfactory conductivity. The latter is further enhanced in an acidic environment and in the presence of TiOs, as it is known that when PANI is doped with HC1 or mixed with certain nanostructured materials such as TiOz and ZnO, its conductivity and electrochemical reversibility over long periods of time are significantly improved. The enhancement of the conductivity of PANI results in the improvement of its anti-fouling ability. Its antibacterial activity is further enriched by long polymer chain lengths, low molecular weights and the presence of amino groups. PANI nanorods are first modified with magnetite nanoparticles and then are properly oriented under an externally applied magnetic field, thus exhibiting high out-of-plane conductivity.
[0041] Magnetic Fe3O4 nanoparticles modify polyniline in order to produce a magnetic nanocomposite capable of being easily oriented in an out of plane configuration under weak magnetic fields. This method promotes the electrical anisotropy of the coating and is particularly advantageous because magnetic forces are contactless.
[0042] The anti-fouling properties of the coating are further enhanced by the incorporation of graphene oxide (GO) sheets in the coating matrix. GO sheets inhibit biofouling through their high conductivity and cytotoxicity, which is due to the generation of reactive oxygen radicals. Their nano sizes reduces raw material requirements and allows for easy dispersion on the carrier. Furthermore, GO sheets provide mechanical reinforcement to the matrix.
[0043] Graphene oxide is modified with TiO?. The latter obtains the crystalline form of the photocatalytically active anatase. Thus, the visible light adsorbed on the surface of the coating leads to the formation of antifouling H2O2. The latter decomposes rapidly into H2O and O2, therefore it is not harmful to the environment. It should be noted, that the large specific surface area of the developed nanostructures makes it possible to develop coatings with small amounts of photocatalysts.
[0044] The binder shall be a water-soluble, non-ionic resin with a high molecular weight of at least 500 000 g / mol. In the present invention a polyethylene oxide resin with a molecular weight of 600,000 g / mol is used. Resins with a higher molecular weight can also be used. The resin used in the present invention has high hardness and toughness. It causes thickening of the water-soluble dispersion, promotes adhesion and provides lubricating and film-forming properties. Its pseudoplastic rheology facilitates the application of the coating without spillage or drift into adjacent areas.
[0045] The composition of the coating takes place in stages, namely: a) Development of the magnetic and electrically conductive PANI / Fe3O4 nanocomposite, which includes the following processes:
[0046] (i) Growth of magnetite (FesCfi) nanoparticles through ultrasonic coprecipitation from Fe divalent and trivalent salts, in the presence of NH3.
[0047] (ii) Development of carboxylic acid-modified aniline dimers.
[0048] (iii) Mixing in an acidic environment and at low temperatures (0-10 °C) the modified aniline and magnetite to produce aniline cores externally decorated with magnetite nanoparticles.
[0049] (iv) Polymerisation of the resulting monomers to obtain polyaniline nanorods (PANI), externally decorated with magnetite nanoparticles. (b) Development of the electrically conductive and photocatalytically active GO / TiCh nanocomposite, which includes the following processes:
[0050] (i) Growth of graphene oxide (GO) sheets, using the modified Hummers method.
[0051] (ii) Ultrasonic growth of a colloidal suspension of the above-grown GO sheets.
[0052] (iii) Mixing in an acidic environment the GO suspension with titanium isopropoxide Ti{OCH(CH3)2}4 to modify the GO sheets with titanium oxide (TiO2) nanoparticles following the crystalline structure of anatase. c) Development of the anti-fouling coating solution, which includes the following processes:
[0053] (i) Development of a nanocomposite mixture by mixing PANI / Fe3O4 and GO / TiO2 nanocomposites in a weight ratio between approximately 1 :1 and approximately 1:4.
[0054] (ii) Dissolving a high viscosity non-ionic polyethene oxide (PEO) resin in water, at a concentration between about 10% w / w and about 55% w / w, preferably between about 20% w / w and about 45% w / w.
[0055] (iii) Addition of the nanocomposite mixture to the aqueous solution of the resin to prepare the final coating solution, wherein the weight ratio of the mixture of nanocomposites and the resin is between about 1:1 and about
[0056] 1 :3. (iv) Addition of pigments, surfactants, adhesion promoters, additives and anti-fouling enhancers. v) Orientation of the PANI / Festli nanocomposite in an out-of-plane configuration under an externally applied magnetic field.
[0057] It was found that magnetic field strengths ranging from 0.01 mT to 0.32 mT were sufficient for the magnetic orientation of the magnetic nanocomposite.
[0058] The final coating solution has a long storage life (over 1 year), without any notable degradation of its anti-fouling properties. It can be applied to various surfaces with common coating techniques (e.g., airless spraying). It should then be allowed to dry at ambient temperature for at least 4 hours.
[0059] It was unexpectedly found that the application of the coating to a naval steel substrate imparted strong anti-fouling properties, which were retained over a long period of time. Unexpectedly, it was also found that the coated surfaces did not develop fouling colonies even after 6 weeks of static immersion in seawater.
[0060] In addition, the coatings exhibit low hydrodynamic resistance under dynamic conditions.
[0061] In addition, it was unexpectedly found that the topcoat could be applied to various substrates without prior surface preparation with a primer. It was further unexpectedly demonstrated through potentiodynamic corrosion curves and Bode and Nyquist impedance plots that the topcoat also imparted corrosion resistant properties to steel substrates without prior surface preparation with an anti-corrosive primer, probably due to the formation of mixed iron oxide layers that provided anodic protection.
[0062] It was found that priming the surface prior to application of the topcoat was not necessary. Nevertheless, the latter seemed to work perfectly well with many of the commercially available antifouling primers.
[0063] The antifouling coating shall be based on a water-soluble matrix and is self-polishing. Its excellent anti-fouling properties are due to different modes of action, which may act individually or in combination. Specifically, the main anti-fouling mechanism is based on the development of a strong three-dimensional conductivity. More specifically, within the coating solution the TiCh-modified sheets of conductive GO are arranged along the in-plane of the dispersed phase. However, the FesO^modified nanorods of conductive PANI are arranged out-of-plane of the dispersed binder due to the magnetic field imposition. Through transmitted electron microscopy, it was unexpectedly found that after the field was removed, the initial orientation of the magnetic nanostructures remained, due to the immobilization of the PANI nanorods by their neighboring ones. Apparently, a high spatial density of modified PANI rods is a prerequisite for the manifestation of this behavior. In contrast, below a critical threshold of PANI concentration, the modified rods cannot maintain the externally imposed orientation.
[0064] It was unexpectedly found that the above geometrical configuration of the nanocomposites is maintained even after the coating is applied to a solid surface. The result is that a high electrical anisotropy develops which imparts strong anti-fouling properties to substrates immersed in water.
[0065] Due to the aforementioned arrangement of nanocomposites, the problem of biofouling is addressed drastically, i.e., at its root, before the onset of primary biofilm formation. In particular, the first stages of colonization are prevented due to the high in-plane conductivity, evoked by the modified GO sheets. The photocatalytically active TiOz further contributes to the inplane anti-fouling ability of the coating. At the same time, the induced electrical anisotropy enhances charge dissipation mechanisms, thus limiting electrostatic attractions and preventing primary adsorption of bacteria and microorganisms through their negatively-charged outer membrane.
[0066] Subsequently, as the coating self-polishes through the gradual dissolution of the carrier, a part of the modified PANI rods becomes exposed and out- of-plane conductivity becomes increasingly important. Colonization is now effectively addressed through the direct contact of microorganisms with the PANI nanorods. Beyond a certain point, the exposure of most of the nanorods makes them flexible, thus allowing microscopic oscillatory movements in the water, which facilitate the detachment of macrofouling under the influence of tidal currents and waves. The manifestation of this mechanism is maximized for a certain range of diameter to length ratios of PANI nanorods, within which their flexibility is enhanced. In this way, a second antifouling defense zone based on foul-release properties is provided, which enhances the primary antifouling properties of the coating and prolongs its useful life. Moreover, an additional mode of antifouling activity is provided when macrofouling has already occurred.
[0067] Through electron microscopy study it was further found that when the diameter-to-length ratio of polyaniline nanorods ranges between 0.0017 and 0.011, their flexibility is maximized and their dirt release properties are enhanced. Within this range, the mechanical strength, elasticity and flexural strength of the coating as well as its out-of-plane conductivity are also improved.
[0068] The electrical conductivity of the nanocomposites was measured by the four-contact method. The ideal conductivity of the GO / TiOz nanocomposite in order for the coating to develop sufficient in-plane antifouling efficacy ranges between 2.06 x 10‘5S / cm and 4.08 x 10'5S / cm. Similarly, the ideal conductivity of PANI / Fe3O4 nanocomposite for developing adequate out-of-plane antifouling efficacy ranges between 1.89 x 10'5S / cm and 3.72 x 10'5S / cm. The 4-contact method was also used to evaluate the electrical anisotropy of the final coating, i.e., the difference between its measured in-plane and out- of-plane conductivity. It was unexpectedly found that the difference in electrical conductivity between the nanocomposites corresponded to the electrical anisotropy of the coating, which indicated that the modified magnetic nanocomposite was oriented almost perpendicular to the coating’s plane.
[0069] The electrical anisotropy of the coating, and thus its anti-fouling ability, is directly dependent on the electrical conductivity of the nanocomposites immediately after their preparation. It is evident that a higher conductivity of the GO / TiO2 nanocomposite compared to the conductivity of the PANI / Fe3O4 nanocomposite promotes the enhancement of the in-plane conductivity, thus preventing early colonization and, consequently, prolonging the coating’s functionality. It was unexpectedly found that the in-plane electrical conductivity of the coating should be at least 5% greater than its out-of-plane electrical conductivity in order to achieve satisfactory anti-fouling performance and prolonged functionality.
[0070] It was also found that the addition of quaternary ammonium salts, e.g., quaternary ammonium silanes, significantly improves the anti-fouling properties of the coating. In this case, the weight ratio between the modified PANI rods and the quaternary ammonium salts should be preferably between 3:1 and 1 :2.
[0071] The binder has a high viscosity. Water-soluble resins with a molecular weight between 500 kDa and 2,000 kDa are considered advantageous.
[0072] The coating provides a chemical "mosaic" with amphiphilic behavior, combining in adjacent heterogeneous nano-regions, the low surface energy of hydrophobic polyaniline with the protein adsorption resistance of hydrophilic TiCf nanoparticles.
[0073] The coating also exhibits strong photocatalytic ability, degrading 73% of the synthetic methylene blue dye after 60 minutes of UV-A irradiation.
[0074] The application of the coatings of the present invention to ships and vessels is cost-effective, not only in terms of maintenance costs, but also in terms of fuel savings and reduction of the time the vessel remains in dry dock. It is also possible to extend the application of the method to other surfaces in contact with water or moisture.
[0075] The production costs of the coatings are relatively low. The cost of application is also low, as on the one hand it is carried out by conventional spraying techniques, and on the other hand it is not necessary to prime the substrate, which allows large surfaces to be coated quickly and economically. The method is therefore industrially feasible.
Claims
CLAIMS1. A method for the development of an electrically conductive and electrically anisotropic coating with high anti -fouling performance and prolonged functionality for solid surfaces in contact with water, comprising: a) a first step of coating the surface with an aqueous dispersion, consisting of: i) a water-soluble resin R with a molecular weight of at least 500,000 g / mol at an amount of between about 10% w / w and about 55% w / w, preferably between about 20% w / w and about 45% w / w; ii) an electrically conductive and photocatalytically active nanocomposite G, having an electrical conductivity between about 2,06 x 10'5S / cm and about 4,08 x 10'5S / cm, consisting of graphene oxide sheets modified with titanium dioxide nanoparticles; iii) a magnetic and electrically conductive nanocomposite P, having an electrical conductivity of between about 1,89 x 10’5S / cm and about 3,72 x 10’5S / cm, consisting of polyaniline nanorods which have a diameter to length ratio of between 0,0017 and 0,011 and which are externally decorated with magnetite nanoparticles; iv) water; and b) a second step of drying the coated surface in air for at least 4 hours.
2. The method according to claim 1, wherein said nanocomposites G and P have a relative (G:P) weight ratio between about 1 : 1 and about 4:1.
3. The method according to claim 1, wherein the mixture (G+P) of said nanocomposites G and P and said resin R have a relative weight ratio((G+P):R) of between about 1:1 and about 1:3.
4. The method according to claim 1 , wherein said magnetic and electrically conductive nanocomposite P is oriented out of the plane of the coating by the imposition of a magnetic field between 0.01 mT and 0.32 mT.
5. The method according to claim 1, wherein the in-plane electrical conductivity of the coating is at least 5% greater than the out-of-plane electrical conductivity of the coating.
Citation Information
Patent Citations
Antifouling paint composition, antifouling coating, substrate with antifouling coating, ?production method thereof, and repair method
EP3831898A1
Electrically conductive antifouling coating composition
US20200231822A1
Waterborne antifouling coating material composition
US20210301153A1
Antifouling coating composition comprising copolymer, method of preparing the copolymer, and antifouling film manufactured from the antifouling coating composition
US20220049112A1
Environmentally Benign Antifouling Coating
US20220332955A1
Cited By
Marine organism fouling inhibiting antifouling paint
JP7936642B1