A method of ammonification modification of ramie fiber and its application method in liquid ammonia solvent dyeing
A ramie fiber modification technology, which is applied in the ammonification modification field of ramie fiber, achieves the effects of reducing environmental pollution, shortening dyeing time, and solving uneven color difference
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2018-09-25
Smart Images

Figure 1 
Figure 2 
Figure 3
Abstract
Description
technical field
[0001] The invention belongs to the technical field of textile chemistry, and in particular relates to an ammonification modification method of ramie fiber and its application method in liquid ammonia solvent dyeing. Background technique
[0002] The textile industry is a traditional pillar industry of my country's national economy and an important livelihood industry. It is also an industry with obvious international competitive advantages. Ramie fiber is one of the main raw materials for textile fabrics and occupies an important position in textile fabrics. my country is one of the countries with the richest hemp resources in the world, mainly including ramie, sisal hemp, flax and jute kenaf, etc. Among them, ramie is widely planted in my country because of its fast growth rate, high yield and easy survival. The fabric made of ramie fiber has the advantages of breathability, moisture absorption and perspiration, and is an ideal summer high-grade clothing fa...
Examples
Embodiment 1
[0026] (1) Pretreatment of ramie fiber: choose ramie yarn for ramie fiber, put 200mL of ramie yarn into 200mL NaOH solution with a concentration of 15%, heat it to 50°C, keep it warm for 4h, and wash it with tap water until the eluate When the pH is 7.6, the pretreated yarn is obtained.
[0027] (2) Modification method: add 10mL formaldehyde, 1mL boric acid and 150mL deionized water into a 250ml three-necked flask, stir evenly, add the 1g ramie yarn after the pretreatment of step (1), and raise the reaction temperature to 40 ℃, then feed ammonia gas, reflux and stir the reaction for 3 hours, after the reaction is completed, take out the yarn, wash it with deionized water, and dry the yarn when the pH of the eluate is 6-7, and the ammoniated modified Sexual ramie yarn.
[0028] (3) Elemental analysis of the modified yarn and the unmodified yarn was performed, and the following results were obtained:
[0029]
[0030] From the elemental analysis results, it can be seen that...
Embodiment 2
[0035] (1) Pretreatment of ramie fiber: choose ramie yarn for ramie fiber, put 200mL of ramie yarn into 200mL NaOH solution with a concentration of 15%, heat it to 50°C, keep it warm for 4h, and wash it with tap water until the eluate When the pH is 7.3, the pretreated yarn is obtained.
[0036] (2) Modification method: add 12mL formaldehyde in 250ml three-necked flask, 1.5mL boric acid and 150mL deionized water, stir evenly, add the 1g ramie yarn after the pretreatment of step (1), temperature of reaction is raised to At 40°C, add ammonia gas, reflux and stir for 3 hours. After the reaction is completed, take out the yarn and rinse it with deionized water. When the pH of the eluate is 6-7, dry the yarn to obtain ammoniated product. Modified ramie yarn.
[0037] (3) Elemental analysis of the modified yarn and the unmodified yarn was performed, and the following results were obtained:
[0038]
[0039] From the elemental analysis results, it can be seen that after the ramie ...
Embodiment 3
[0044] (1) Pretreatment of ramie fiber: choose ramie yarn for ramie fiber, put 200mL of ramie yarn into 200mL NaOH solution with a concentration of 15%, heat it to 50°C, keep it warm for 4h, and wash it with tap water until the eluate When the pH is 7.1, the pretreated yarn is obtained.
[0045] (2) Modification method: add 12mL formaldehyde in 250ml three-necked flask, 1.5mL boric acid and 150mL deionized water, stir evenly, add the 1g ramie yarn after the pretreatment of step (1), temperature of reaction is raised to At 40°C, add ammonia gas, reflux and stir for 3 hours. After the reaction is completed, take out the yarn and rinse it with deionized water. When the pH of the eluate is 6-7, dry the yarn to obtain ammoniated product. Modified ramie yarn.
[0046] (3) Elemental analysis of the modified yarn and the unmodified yarn was performed, and the following results were obtained:
[0047]
[0048] From the elemental analysis results, it can be seen that after the rami...