A high-quality, pyrite technology, applied in chemical instruments and methods, wet separation, solid separation, etc., can solve the problem that iron minerals cannot be dissociated individually, the recovery rate of iron minerals is not high, and the grinding cost is increased. and other issues, to achieve strong guiding significance and reference value, improve corporate and social economic benefits, and be easy to operate.
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2017-03-08
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention belongs to the technical field of pyrite, and specifically refers to a method for recovering high-quality iron ore from pyrite with high sulfur content. Background technique
[0002] The ore processed by some mines is high sulfur refractory iron ore. The iron minerals and sulfur minerals in the ore are mainly inlaid with medium and fine grains, and some are inlaid with coarse grains. They fill and replace each other along the fissures of each other in a veinlet shape, and it is difficult to completely dissociate the monomers during the grinding process, which has a certain impact on the flotation recovery of iron and sulfur.
[0003] The particle size of iron and sulfur mineral intercalation is uneven, the particle size of iron mineral intercalation is relatively fine, and the particle size of sulfur mineral intercalation is relatively coarse. Some iron minerals and sulfur minerals are closely combined. If the grinding size is too coars...
Examples
Embodiment 1
[0021] A method for reclaiming high-quality iron ore from pyrite with high sulfur content comprises the following steps:
[0022] (1) Crush and grind the raw ore to 200 mesh, then add agent A to continue grinding to 400 mesh, and keep the temperature at 75°C, agent A is benzothiazole mercaptan, benzimidazole mercaptan and benzoxazole mercaptan The mixture, the weight ratio of benzothiazole thiol, benzimidazole thiol and benzoxazole thiol is 1:1:3;
[0023] (2) Add water to the mineral material obtained in step (1) to adjust the concentration of the flotation pulp to 36%, add collector B, the amount of arsenate added is 2wt% of the pulp, stir for 5-7min, and then send it to the flotation machine Internal flotation for 10 minutes to obtain mixed concentrate of iron and sulfur, collector B uses arsenic acid ester;
[0024] (3) Add 300g / t of carbon powder and lime water to the iron-sulfur mixed concentrate in step (2) to adjust the pH of the slurry to 12.3 or above, stir for 5 mi...
Embodiment 2
[0028] A method for reclaiming high-quality iron ore from pyrite with high sulfur content comprises the following steps:
[0029] (1) Crush and grind the raw ore to 300 mesh, then add agent A to continue grinding to 500 mesh, and keep the temperature at 75-85°C, agent A is benzothiazole mercaptan, benzimidazole mercaptan and benzoxazole Thiol mixture, the weight ratio of benzothiazole thiol, benzimidazole thiol and benzoxazole thiol is 1:1:3;
[0030] (2) Add water to the mineral material obtained in step (1) to adjust the concentration of the flotation pulp to 37%, add collector B, the amount of arsenate added is 5wt% of the pulp, stir for 7 minutes, and send it to the flotation machine for flotation After 15 minutes, the mixed concentrate of iron and sulfur can be obtained, and the collector B adopts arsenic acid ester;
[0031] (3) Add 800g / t of carbon powder and lime water to the iron-sulfur mixed concentrate in step (2) to adjust the pH of the slurry to above 12.3, stir ...
Embodiment 3
[0035] A method for reclaiming high-quality iron ore from pyrite with high sulfur content comprises the following steps:
[0036] (1) Crush and grind the raw ore to 260 mesh, then add agent A to continue grinding to 470 mesh, and keep the temperature at 80°C, agent A is benzothiazole mercaptan, benzimidazole mercaptan and benzoxazole mercaptan The mixture, the weight ratio of benzothiazole thiol, benzimidazole thiol and benzoxazole thiol is 1:1:3;
[0037] (2) Add water to the mineral material obtained in step (1) to adjust the concentration of the flotation pulp to 36%, add collector B, the amount of arsenate added is 3wt% of the pulp, stir for 6 minutes, and send it to the flotation machine for flotation After 12 minutes, the mixed concentrate of iron and sulfur can be obtained, and the collector B adopts arsenic acid ester;
[0038] (3) Add 500g / t of carbon powder and lime water to the iron-sulfur mixed concentrate in step (2) to adjust the pH of the slurry to above 12.3, ...