A SPE membrane electrode and its preparation process
By using polyester frames instead of the blank area of the proton exchange membrane in the SPE electrolytic membrane electrode, and using large proton exchange membrane spraying catalysts on the whole surface, the low utilization rate of the membrane electrode and catalyst are solved by using the membrane electrode. The problem of low spraying efficiency improves the production efficiency and connection strength of the membrane electrodes, and releases the production capacity potential of SPE electrolytic cells.
Patent Information
- Application Number
- CN201710871948.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-09-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2037-09-25
Smart Images

Figure CN107604379B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of SPE water electrolysis hydrogen production, and in particular to a SPE membrane electrode and a preparation process thereof. Background Art
[0002] Hydrogen energy is the most ideal energy source in the future. Hydrogen production by water electrolysis has broad development prospects. SPE water electrolysis hydrogen production, namely Solid Polymer Electrolyte water electrolysis hydrogen production, is called solid polymer electrolyte water electrolysis hydrogen production technology. The core of this technology is the solid polymer electrolyte electrolytic cell, as shown in the attached Figure 5 As shown, the SPE electrolytic cell generally comprises a membrane electrode 100, a bipolar plate 200, an end plate 300 and a sealing gasket 400, etc. The bipolar plates 200 are arranged on both sides of the membrane electrode 100, and the membrane electrode 100 and the bipolar plates 200 are fixedly connected by fasteners or the like. Among them, the membrane electrode 100 is one of the core components of the SPE electrolytic cell and determines the performance of the SPE electrolytic cell.
[0003] The membrane electrode 100 is to embed active electrodes on both sides of the solid polymer electrolyte membrane, so that the membrane and the electrode become a whole, and the electrochemical reaction of water is carried out in it, which is equivalent to the role of the diaphragm and the electrode. The solid polymer electrolyte membrane is usually a proton exchange membrane, and its full name is perfluorosulfonic acid proton exchange membrane. It is a tough, soft perfluorinated sulfonic acid polymer sheet with high conductivity to hydrogen ions; the active electrode is a solid catalyst, which is generally a platinum metal and its oxide, and the cathode oxidant and the anode oxidant are embedded on the opposite sides of the proton exchange membrane, and the compositions of the cathode oxidant and the anode oxidant are different. The typical structure of the membrane electrode 100 is as follows: Figure 6 As shown, it includes a proton exchange membrane 10 and a catalyst 20; the catalyst 20 is prepared and formulated into a suspension, and is directly sprayed on the middle of the proton exchange membrane by a robot or other equipment, the area where the catalyst 20 is located forms a catalytically effective area 11, and the area on the proton exchange membrane 10 that is not covered with the catalyst forms a blank area 12, the peripheral shape and size of the blank area 12 are adapted to the bipolar plate 200, and the periphery extends inwardly, so that the blank area 12 has a certain width, so that fasteners are arranged on it and connected to the bipolar plate 200. The membrane electrode 100 as described above has at least the following disadvantages during the manufacturing process:
[0004] 1. When the proton exchange membrane is made into a membrane electrode assembly, only the middle part becomes an effective catalytic area, the utilization rate of the proton exchange membrane is low, and the amount used is large;
[0005] 2. In order to ensure the area of the blank area, the catalyst needs to be sprayed with great care, especially at the junction of the blank area and the effective catalytic area. The spraying process takes a long time, has a low tolerance rate, and low production efficiency;
[0006] 3. Because the catalyst is a prepared suspension, and the amount of a single proton exchange membrane is not large, and the spraying time is too long due to the disadvantage 2, if too much catalyst is prepared, the unused part is prone to sedimentation, which is not suitable for large-capacity catalyst preparation. It can only be prepared one by one, which is time-consuming and laborious;
[0007] 4. The membrane electrode production efficiency and output are low, which seriously restricts the overall output efficiency of the SPE electrolytic cell and becomes a major pain point and bottleneck in the production of SPE electrolytic cells. Summary of the invention
[0008] The purpose of the present invention is to provide a membrane electrode of SPE water electrolysis technology, which can overcome the shortcomings of the prior art, not only significantly improve the utilization rate of proton exchange membrane, reduce the use of proton exchange membrane, but also reduce the cost of membrane electrode, and ensure and improve the connection strength between membrane electrode and bipolar plate.
[0009] Another object of the present invention is to provide a membrane electrode preparation process for SPE water electrolysis technology, which can overcome the shortcomings of the prior art, greatly improve the catalyst spraying efficiency and membrane electrode manufacturing efficiency, and fully release the production capacity potential of the SPE electrolytic cell.
[0010] The above technical objectives of the present invention are achieved through the following technical solutions:
[0011] A SPE membrane electrode is installed in an SPE electrolytic cell including the membrane electrode, bipolar plates, end plates, and sealing gaskets. The membrane electrode includes a proton exchange membrane, a catalyst embedded in the proton exchange membrane, and a polyester frame surrounding the outer edge and responsible for connecting with the bipolar plate.
[0012] Only a very narrow portion of the outer edge of the proton exchange membrane is left blank for combination with the polyester frame, so that most of the area of the proton exchange membrane is used to embed the catalyst. The used area of the proton exchange membrane in a single membrane electrode is greatly reduced, and the utilization rate is greatly improved. The task of connecting the membrane electrode and the bipolar plate is handed over to the cheaper and harder polyester frame, rather than leaving a large area on the expensive proton exchange membrane for mechanical connection. This greatly reduces the manufacturing cost of the membrane electrode while ensuring the same effective area of the catalyst, and the connection strength is higher.
[0013] Preferably, the proton exchange membrane comprises a loading area for embedding the catalyst, and a non-loading area located at the edge of the loading area for connecting with the polyester frame.
[0014] The loading area is used to embed the catalyst as a catalytically effective area, and the unloaded area has no catalyst embedded in it and is left blank for combining with the polyester frame. The combining method can be hot pressing.
[0015] Preferably, the polyester frame includes a polyester frame substrate whose edge is adapted to the shape and size of the bipolar plate, an inner frame opened in the middle of the polyester frame substrate for placing the proton exchange membrane, and a through cavity opened in the middle of the inner frame for exposing the catalyst to the outside.
[0016] The depth of the inner frame is adapted to half the thickness of the unloaded area, so that the inner frame after the two polyester frames are bonded together forms a complete accommodating area that adapts to the thickness of the unloaded area. The area in the inner frame where the through cavity is not opened is used for physical contact with the unloaded area, and its width is consistent with the shape and size of the unloaded area.
[0017] Preferably, the number of the polyester frames is two, and the two polyester frames are attached together in a mirror-symmetrical manner to accommodate the proton exchange membrane.
[0018] When the two ester frames are attached together, their respective inner frames are also joined together to form a space for accommodating a complete proton exchange membrane.
[0019] Preferably, the distance between the outer surface of the catalyst and the center of the proton exchange membrane is smaller than the distance between the outer surface of the polyester frame on the same side after being bonded together and the center of the proton exchange membrane.
[0020] Therefore, after the polyester frame is combined with the proton exchange membrane, the thickest part of the membrane electrode is the polyester frame area, and the surface of the catalytic active area is within the polyester frame, thereby better protecting the surface of the catalytic active area during subsequent processing, packaging, and component installation.
[0021] Preferably, the width of the joining portion between the proton exchange membrane and the polyester frame is 5 mm.
[0022] The blank portion in the proton exchange membrane is made much smaller than the blank portion used for connecting the bipolar plates in the prior art, thereby greatly improving the utilization rate of the proton exchange membrane.
[0023] Preferably, the end surface of the polyester frame is 0.05 mm higher than the catalyst.
[0024] A SPE membrane electrode preparation process comprises the following steps:
[0025] A) Catalyst spraying preparation: after removing organic and inorganic impurities on the proton exchange membrane, the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape or the like;
[0026] The width of the tape at the edge of the proton exchange membrane is not less than the width of the joining portion of the proton exchange membrane and the polyester frame, and the width of the tape outside the edge of the proton membrane is not less than twice the width of the joining portion of the proton exchange membrane and the polyester frame, so that when the catalyst spraying is completed and cut into a single proton exchange membrane, the area covered by the tape can be smoothly cut into the width for combining with the polyester frame. The adhesion of the tape can be achieved by making special adhesion tooling, which is convenient and quick, and the catalyst sprayed on the tape can be recycled and reused.
[0027] B) Catalyst spraying: Prepare the catalyst, use a spraying device to evenly spray the catalyst onto the entire proton exchange membrane, and let it stand to dry after spraying;
[0028] The unloaded area is covered by tape, so there is no concern about the existence of unsprayed areas when the catalyst is sprayed, the spraying process is simplified and the time is greatly shortened; the entire proton exchange membrane is sprayed at the same time, which greatly reduces the number of preparations for spraying a single proton exchange membrane, greatly improves the spraying efficiency, and the catalyst can also be prepared in large quantities and used together. The preparation time of the catalyst is also greatly shortened, avoiding the dilemma of having to prepare and use the catalyst immediately when spraying a single proton exchange membrane.
[0029] C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area;
[0030] Thus, multiple proton exchange membranes with smaller areas and catalytic effective areas that meet the requirements can be produced by spraying at one time, the utilization rate of the proton exchange membranes is greatly improved, and material waste is reduced.
[0031] D) Preparation for hot pressing: Use high temperature adhesive tape to place the single proton exchange membrane treated in step C between the two polyester frames, with the catalytic active area completely exposed outside the surface covering area of the polyester frame, and the area where the two polyester frames are joined is evenly coated with hot pressing adhesive;
[0032] The high-temperature tape can be a polyimide tape, and the proton exchange membrane is fixed between two polyester frames by the polyimide tape, so that the connection position is stable and prevented from loosening; the hot pressing adhesive melts under high temperature and hot pressure, and then a certain pressure is applied to the two polyester frames for a period of time, and the polyester frames are bonded together.
[0033] E) Hot pressing: the membrane electrode coated with the flexible graphite plate treated in step D is placed in two heating plates of a hydraulic press, hot pressed at a set pressure and temperature for a set time, and then the membrane electrode is taken out and left to cool;
[0034] The flexible graphite plate acts as a pressure buffer to make the hot pressing pressure on the membrane electrode more uniform and prevent the membrane electrode from deforming.
[0035] F) Post-processing: taking out the membrane electrode from the hydraulic press, leaving it to cool, and removing the flexible graphite sheet coated on the membrane electrode in step E and the high-temperature tape in step D.
[0036] Preferably, the width of the joining portion between the proton exchange membrane and the polyester frame is 2 to 7 mm.
[0037] Preferably, the width of the tape at the edge of the proton exchange membrane in step A is not less than the width of the joining portion between the proton exchange membrane and the polyester frame, and the width of the tape outside the edge of the proton exchange membrane is not less than twice the width of the joining portion between the proton exchange membrane and the polyester frame.
[0038] Preferably, the hot pressing time in step E is 6 to 15 minutes, the hot pressing temperature is 110° C. to 130° C., and the hot pressing pressure is 15 to 25 MPa.
[0039] Preferably, in step E, the surface of the membrane electrode is also coated with a PTFE plate.
[0040] Flexible graphite sheets and PTFE sheets are wrapped in sequence to form better pressure buffering.
[0041] In summary, the present invention has the following beneficial effects:
[0042] A SPE membrane electrode seals and connects a proton exchange membrane embedded with a catalyst through a polyester frame, that is, the polyester frame is used to replace the blank area on the large proton exchange membrane in the prior art to connect the bipolar plates in the electrolytic cell. The polyester frame has high strength and low price, and the blank area on the proton exchange membrane is greatly reduced. Under the premise of ensuring the overall size of the membrane electrode and the original catalytic effective area, the amount of expensive proton exchange membrane in a single membrane electrode is greatly reduced, the utilization rate of the proton exchange membrane is significantly improved, and the connection between the membrane electrode and the bipolar plate is made stronger and more reliable, thereby greatly reducing the production cost of the membrane electrode.
[0043] A SPE membrane electrode preparation process uses a large proton exchange membrane to spray the catalyst on the entire surface at the same time, and then cuts out individual proton exchange membranes of required size, leaving an extremely narrow area of width in contact with the polyester frame. This greatly improves the efficiency of catalyst spraying, reduces the number of spray preparations, greatly increases the amount of catalyst used in one spray, reduces the number of catalyst preparations, greatly improves the production efficiency of membrane electrodes, and solves the bottleneck of low membrane electrode output and long manufacturing time in electrolytic cell production, greatly releasing production capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a schematic diagram of the structure of the SPE membrane electrode of the present invention;
[0045] Figure 2 It is a schematic diagram of the structure of the proton exchange membrane of the present invention;
[0046] Figure 3 It is a schematic diagram of the structure of the polyester frame;
[0047] Figure 4 This is a schematic diagram of the structure after the entire proton exchange membrane is sprayed with catalyst;
[0048] Figure 5 is a schematic diagram of the structure of an electrolytic cell;
[0049] Figure 6 It is a schematic diagram of the structure of a membrane electrode in the prior art. DETAILED DESCRIPTION
[0050] The present invention is further described in detail below in conjunction with the accompanying drawings and preferred solutions.
[0051] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
[0052] Example 1: Figure 1-3 As shown, an SPE membrane electrode is installed in an SPE electrolytic cell including a membrane electrode 100, a bipolar plate 200, an end plate 300, and a sealing gasket 400. The membrane electrode 100 includes a proton exchange membrane 10, a catalyst 20 embedded in the proton exchange membrane 10, and a polyester frame 30 surrounding the outer edge and responsible for connecting with the bipolar plate 200.
[0053] The proton exchange membrane 10 includes a loading area 13 for embedding a catalyst 20 , and a non-loading area 14 located at the edge of the loading area 13 for connecting with a polyester frame 30 .
[0054] The polyester frame 30 includes a polyester frame substrate 31 whose edge is adapted to the shape and size of the bipolar plate 200, an inner frame 32 opened in the middle of the polyester frame substrate 31 for placing the proton exchange membrane 10, and a through cavity 33 opened in the middle of the inner frame 32 for exposing the catalyst 20 to the outside.
[0055] There are two polyester frames 30 , which are attached together in a mirror-symmetrical manner and contain the proton exchange membrane 10 .
[0056] The distance between the outer surface of the catalyst 20 and the center of the proton exchange membrane 10 is smaller than the distance between the outer surface of the polyester frame 30 on the same side and the center of the proton exchange membrane 10 after being bonded together.
[0057] The width of the joint portion between the proton exchange membrane and the polyester frame is 5 mm.
[0058] The end surface of the polyester frame is 0.05 mm higher than the catalyst.
[0059] The size of the proton exchange membrane is 73mmX73mm.
[0060] The size of the SPE membrane electrode is 110 mm x 110 mm.
[0061] Example 2: Figure 1 , 4 As shown, a SPE membrane electrode preparation process includes the following steps:
[0062] A) Catalyst spraying preparation: After removing organic and inorganic impurities on the proton exchange membrane 10, the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape or the like;
[0063] B) Catalyst spraying: Prepare the catalyst 20, use a spraying device to evenly spray the catalyst 20 onto the entire proton exchange membrane, and let it stand to dry after spraying;
[0064] C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area;
[0065] D) Preparation for hot pressing: Use high temperature adhesive tape to place the single proton exchange membrane treated in step C between two polyester frames 30, with the catalytic active area completely exposed outside the surface covering area of the polyester frame 30, and the area where the two polyester frames 30 are joined is evenly coated with hot pressing adhesive;
[0066] E) Hot pressing: The membrane electrode 100 treated in step D is coated with a flexible graphite plate and then placed in two heating plates of a hydraulic press. The membrane electrode is hot pressed at a set pressure and temperature for a set time, and then the membrane electrode is taken out and left to cool;
[0067] F) Post-processing: Take out the membrane electrode 100 from the hydraulic press, let it stand and cool, and remove the flexible graphite sheet coated on the membrane electrode 100 in step E and the high-temperature tape in step D.
[0068] The width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30 is 5 mm.
[0069] In step A, the width of the tape at the edge of the proton exchange membrane 10 is consistent with the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30, and the width of the tape outside the edge of the proton exchange membrane 10 is consistent with twice the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30.
[0070] The hot pressing time in step E is 10 minutes, the hot pressing temperature is 115° C., and the hot pressing pressure is 20 MPa.
[0071] Example 3: Figure 1 , 4 As shown, a SPE membrane electrode preparation process includes the following steps:
[0072] A) Catalyst spraying preparation: After removing organic and inorganic impurities on the proton exchange membrane 10, the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape or the like;
[0073] B) Catalyst spraying: Prepare the catalyst 20, use a spraying device to evenly spray the catalyst 20 onto the entire proton exchange membrane, and let it stand to dry after spraying;
[0074] C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area;
[0075] D) Preparation for hot pressing: Use high temperature adhesive tape to place the single proton exchange membrane treated in step C between two polyester frames 30, with the catalytic active area completely exposed outside the surface covering area of the polyester frame 30, and the area where the two polyester frames 30 are joined is evenly coated with hot pressing adhesive;
[0076] E) Hot pressing: The membrane electrode 100 treated in step D is coated with a flexible graphite plate and then placed in two heating plates of a hydraulic press. The membrane electrode is hot pressed at a set pressure and temperature for a set time, and then the membrane electrode is taken out and left to cool;
[0077] F) Post-processing: Take out the membrane electrode 100 from the hydraulic press, let it stand and cool, and remove the flexible graphite sheet coated on the membrane electrode 100 in step E and the high-temperature tape in step D.
[0078] The width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30 is 5 mm.
[0079] In step A, the width of the tape at the edge of the proton exchange membrane 10 is equal to the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30, and the width of the tape outside the edge of the proton exchange membrane 10 is equal to twice the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30.
[0080] The hot pressing time in step E is 10 minutes, the hot pressing temperature is 120° C., and the hot pressing pressure is 20 MPa.
[0081] The membrane electrode surface is also coated with a PTFE sheet.
[0082] Example 4: Figure 1 , 4 As shown, a SPE membrane electrode preparation process includes the following steps:
[0083] A) Catalyst spraying preparation: After removing organic and inorganic impurities on the proton exchange membrane 10, the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape or the like;
[0084] B) Catalyst spraying: Prepare the catalyst 20, use a spraying device to evenly spray the catalyst 20 onto the entire proton exchange membrane, and let it stand to dry after spraying;
[0085] C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area;
[0086] D) Preparation for hot pressing: Use high temperature adhesive tape to place the single proton exchange membrane treated in step C between two polyester frames 30, with the catalytic active area completely exposed outside the surface covering area of the polyester frame 30, and the area where the two polyester frames 30 are joined is evenly coated with hot pressing adhesive;
[0087] E) Hot pressing: The membrane electrode 100 treated in step D is coated with a flexible graphite plate and then placed in two heating plates of a hydraulic press. The membrane electrode is hot pressed at a set pressure and temperature for a set time, and then the membrane electrode is taken out and left to cool;
[0088] F) Post-processing: Take out the membrane electrode 100 from the hydraulic press, let it stand and cool, and remove the flexible graphite sheet coated on the membrane electrode 100 in step E and the high-temperature tape in step D.
[0089] The width of the joint between the proton exchange membrane 10 and the polyester frame 30 is 7 mm.
[0090] In step A, the width of the tape at the edge of the proton exchange membrane 10 is equal to the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30, and the width of the tape outside the edge of the proton exchange membrane 10 is equal to twice the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30.
[0091] The hot pressing time in step E is 6 minutes, the hot pressing temperature is 110° C., and the hot pressing pressure is 15 MPa.
[0092] In step E, the surface of the membrane electrode is also coated with a PTFE plate.
[0093] Example 5: Figure 1 , 4 As shown, a SPE membrane electrode preparation process includes the following steps:
[0094] A) Catalyst spraying preparation: After removing organic and inorganic impurities on the proton exchange membrane 10, the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape or the like;
[0095] B) Catalyst spraying: Prepare the catalyst 20, use a spraying device to evenly spray the catalyst 20 onto the entire proton exchange membrane, and let it stand to dry after spraying;
[0096] C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area;
[0097] D) Preparation for hot pressing: Use high temperature adhesive tape to place the single proton exchange membrane treated in step C between two polyester frames 30, with the catalytic active area completely exposed outside the surface covering area of the polyester frame 30, and the area where the two polyester frames 30 are joined is evenly coated with hot pressing adhesive;
[0098] E) Hot pressing: The membrane electrode 100 treated in step D is coated with a flexible graphite plate and then placed in two heating plates of a hydraulic press. The membrane electrode is hot pressed at a set pressure and temperature for a set time, and then the membrane electrode is taken out and left to cool;
[0099] F) Post-processing: Take out the membrane electrode 100 from the hydraulic press, let it stand and cool, and remove the flexible graphite sheet coated on the membrane electrode 100 in step E and the high-temperature tape in step D.
[0100] The width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30 is 2 mm.
[0101] In step A, the width of the tape at the edge of the proton exchange membrane 10 is equal to the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30, and the width of the tape outside the edge of the proton exchange membrane 10 is equal to twice the width of the bonding portion between the proton exchange membrane 10 and the polyester frame 30.
[0102] The hot pressing time in step E is 15 minutes, the hot pressing temperature is 130° C., and the hot pressing pressure is 25 MPa.
[0103] In step E, the surface of the membrane electrode is also coated with a PTFE plate.
Claims
1. A method for preparing a SPE membrane electrode, characterized in that: The following steps are involved: A) Catalyst spraying preparation: After removing organic and inorganic impurities on the proton exchange membrane (10), the whole proton exchange membrane is fixedly clamped on the spraying station, and the whole proton exchange membrane is divided into proton exchange membranes having an integer number of catalytically effective areas in a single proton exchange membrane by means of adhesive tape; B) Catalyst spraying: After the catalyst (20) is prepared, the catalyst (20) is evenly sprayed onto the entire proton exchange membrane using a spraying device, and after the spraying is completed, the catalyst is allowed to stand and dry; C) Proton exchange membrane cutting: tear off the tape used in step A, and cut the entire proton exchange membrane treated in step B into multiple single proton exchange membranes based on the unsprayed area; D) Preparation for hot pressing: using a high temperature adhesive tape, place the single proton exchange membrane after the treatment in step C between two polyester frames (30) in the center, with the catalytic active area completely exposed outside the surface coverage area of the polyester frame (30), and the area where the two polyester frames (30) are joined is evenly coated with hot pressing adhesive to form a membrane electrode (100); E) Hot pressing: a flexible graphite sheet is coated on the surface of the membrane electrode (100), and then placed in two heating plates of a hydraulic press, and hot pressed at a set pressure value and temperature for a set time, after which the membrane electrode is taken out and left to cool; F) Post-treatment: Take out the membrane electrode from the hydraulic press, let it stand and cool, remove the flexible graphite sheet coated on the membrane electrode in step E and the high-temperature tape in step D, and obtain the SPE membrane electrode.
2. The preparation method according to claim 1, characterized in that: The width of the joint portion between the proton exchange membrane (10) and the polyester frame (30) is 2 to 7 mm.
3. The preparation method according to claim 1, characterized in that: In step A), the width of the adhesive tape at the edge of the proton exchange membrane (10) is not less than the width of the junction between the proton exchange membrane (10) and the polyester frame (30), and the width of the adhesive tape at the portion other than the edge of the proton exchange membrane (10) is not less than twice the width of the junction between the proton exchange membrane (10) and the polyester frame (30).
4. The preparation method according to claim 1, characterized in that: In step E), the hot pressing time is 6 to 15 minutes, the hot pressing temperature is 110° C. to 130° C., and the hot pressing pressure is 15 to 25 MPa.
5. The preparation method according to claim 1, characterized in that: In step E), after the surface of the membrane electrode (100) is coated with the flexible graphite sheet, it is also coated with a PTFE sheet.