Methods for Improving the Quality of Steel Ingots for Bridges
By optimizing the flow field and cooling process of continuous casting, combined with liquid core pressure and electromagnetic stirring technology, the problem of low quality of casting billets in bridge steel production is solved, the quality and qualification rate of casting billets are improved, and the production is reduced cost.
Patent Information
- Application Number
- CN201710773736.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-08-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2037-08-31
AI Technical Summary
The existing bridge steel production process is difficult to take into account the high strength, high toughness and low yield and strength ratio and excellent Z-directional properties of steel plates, resulting in low quality of cast billets, prone to loose centers, corner defects and large inclusions exceeding the standard, which has increased Production cost.
By optimizing the continuous casting tundra flow field and second-cold section cooling process, combining liquid core pressure and electromagnetic stirring technology, the cooling water volume and protective slag layer are controlled, the impact of the crystallizer wall is reduced, the contact between the protective slag and the liquid steel is improved, and the inclusion is enhanced. The removal rate of the object is adopted, and the full-pack control and slag retaining wall settings are used to optimize the middle-pack flow field and the four-hole outlet flow field.
It significantly improves the quality and qualification rate of steel casting billets for bridges, reduces production costs, solves the problems of loose centers, corner defects and inclusions exceeding the standard, and ensures the quality and performance of the surface and core of the casting billet.
Smart Images

Figure CN107626902B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to metallurgical technology, in particular to a method for improving the quality of steel castings for bridges. Background Art
[0002] While pursuing high strength and high toughness, bridge steel takes yield strength ratio as an important performance indicator. A low yield strength ratio of steel means that the steel structure has a high hardening index and high uniform elongation, which is generally achieved by controlling the cooling process. The soft and hard aspects of the organization are taken into account, but the process window is very narrow, and the Z-direction performance of the steel plate must also be taken into account. Therefore, the quality of the original steel billet is very important for the quality control of the next process. The fewer inclusions inside the billet, the lower the degree of segregation, and the less gas content, the more conducive it is to obtain a lower yield strength ratio, high toughness and plasticity, and thickness direction performance after controlled rolling and controlled cooling in the next process, and at the same time improve the qualified rate of flaw detection after rolling of the steel plate. However, the current bridge steel production process is difficult to take into account the low yield strength ratio and the Z-direction performance of the steel plate while obtaining high strength and high toughness, which leads to problems such as low billet quality, loose center of continuous casting billet, easy corner defects, and excessive large inclusions in the billet, which increases production costs.
[0003] Chinese patent application CN 105506450 A discloses an earthquake-resistant and weather-resistant bridge steel and a manufacturing process thereof, wherein the earthquake-resistant and weather-resistant bridge steel comprises the following components by weight percentage: C: 0.04-0.08%, Si: 0.15-0.30%, Mn: 0.80-1.50%, P≤0.010%, S≤0.008%, Cu: 0.20-0.45%, Cr: 0.30-0.50%, Ni: 0.25-0.50%, Nb: 0.02-0.04%, V: 0.005-0.0.05%, Ti: 0.008-0.020% , Alt: 0.02-0.05%, the rest is Fe. The invention has simple process, low cost, high strength, high toughness and excellent welding performance, can meet the needs of large thickness and wide specification modern bridge structure construction, low carbon content and carbon equivalent design, adding a small amount of Nb and V, reducing the alloy cost, and obtaining fine grain structure through controlled rolling and controlled cooling. It has a yield ratio of ≤0.80, high strength, high toughness and excellent weldability, which can meet the requirements of low yield ratio, but the Z-direction performance cannot be met, with a single value less than 25, the ingot is prone to defects and the quality is not high. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the quality of steel ingots for bridges, which improves the quality and pass rate of the ingots and reduces the production cost.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a method for improving the quality of steel ingots for bridges, comprising smelting, continuous casting, heating and cooling steps, in which the temperature of the tundish is controlled within the liquidus range of 15 to 20°C, and the pulling speed is controlled at 0.8 to 0.9 m / min; in the cooling step, water is distributed in the second cooling section: the cooling water volume of the full roll section is 80 to 230 L / min, the cooling water volume of the vertical section is 60 to 120 L / min, the water volume of the outer arc of the bending section is 45 to 55 L / min, the water volume of the inner arc of the bending section is 30 to 40 L / min, the cooling water volume of the outer arc of the straightening section is 75 to 80 L / min, and the cooling water volume of the inner arc of the straightening section is 45 to 50 L / min.
[0006] Furthermore, in the continuous casting step, a liquid core pressing process is adopted for the solidification end and electromagnetic stirring is used for continuous casting into a slab.
[0007] Furthermore, in the continuous casting step, the liquid core is pressed down by 5 to 10 mm, the electromagnetic stirring current is 440 to 460 A, and the frequency is 5 to 8 Hz.
[0008] Furthermore, in the continuous casting step, the middle ladle is controlled to be full at 35 to 45 tons, and a slag retaining wall and a slag retaining dam are provided in the middle ladle. The middle wall height of the slag retaining wall is 1020 to 1030 mm, the upper width is 1900 to 2000 mm, the lower width is 1580 to 1600 mm, and the outer side is inclined by 10 to 15° in the horizontal direction; the slag retaining dam is 250 to 350 mm high, forming an angle of 75 to 80° with the slag retaining wall, and the double drainage outlets are symmetrically distributed, and the water inlet insertion depth is 120 to 160 mm.
[0009] Furthermore, the slag retaining wall of the middle ladle is provided with two square holes in a single row, and two round holes are respectively opened on the two side walls of the middle ladle.
[0010] Furthermore, in the cooling step, the solidification end is 18.50 to 19.50 m away from the liquid surface of the crystallizer.
[0011] Furthermore, in the continuous casting step, the thickness of the liquid slag layer of the continuous casting crystallizer protection slag is controlled to be 6 to 10 mm, the basicity of the liquid slag is controlled to be 0.65 to 0.68 mm, and the viscosity is controlled to be 0.43 to 0.46 Pa·s.
[0012] Compared with the prior art, the present invention has the following advantages:
[0013] Firstly, the method of the present invention optimizes the flow field of the tundish during continuous casting and cooperates with the corresponding cooling process of the secondary cooling section to improve the quality of the steel ingots for bridges, solve the problems of looseness in the center of the continuous casting ingots, corner defects, and failure of nondestructive testing caused by excessive large inclusions in the ingots, thereby greatly reducing production costs.
[0014] Secondly, during continuous casting, the method of the present invention optimizes the flow field of the tundish and cooperates with the four-hole water nozzle flow field to weaken the impact on the crystallizer wall and reduce the impact depth, thereby increasing the contact between the protective slag and the molten steel, giving full play to the ability of the protective slag for bridge steel to absorb inclusions, improving the removal rate of inclusions in the continuous casting process, and is beneficial to further improving the quality of bridge steel ingots.
[0015] Thirdly, the electromagnetic stirring and liquid core pressing technology in the present invention cooperates with the corresponding secondary cooling process to ensure the quality of the surface and core of the ingot. After sampling and analysis, the ingot has no obvious looseness or shrinkage holes, and no edge cracks at the corners. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the quality of the bridge steel ingot obtained in Example 1.
[0017] Figure 2 This is a picture of steel ingots used in existing bridges. DETAILED DESCRIPTION
[0018] The present invention will be further described in detail below in conjunction with specific embodiments to facilitate a clearer understanding of the present invention, but they do not limit the present invention.
[0019] Example 1
[0020] 1) Smelting and continuous casting: conventional smelting, control the temperature of the upper continuous casting platform, during continuous casting, control the temperature of the tundish to be 15°C higher than the liquidus (liquidus temperature is 1511-1524°C), the pulling speed is controlled at 0.83m / min, and the solidification end dynamic soft pressure is adopted and electromagnetic stirring technology is used to continuously cast into 230*2150mm slabs, among which the liquid core is pressed down by 5mm, the electromagnetic stirring current is 450A, and the frequency is 6HZ; the tundish adopts full bag control, and the control It is made in 40 tons, and the middle package is equipped with a slag retaining wall and a slag retaining dam. The middle wall height of the slag retaining wall is 1020mm, the upper width is 1900mm, the lower width is 1580mm, and there are two square holes in a single row. The size of the square holes is 120*120mm, and the outer side is inclined 11° in the horizontal direction. Two circular holes with a diameter of 80mm are opened on each side wall; the slag retaining dam is 250mm high and forms a 75° angle to the slag retaining wall. The double drainage outlets are symmetrically distributed, and the water inlet insertion depth is 120mm.
[0021] 2) Cooling water configuration: The water volume of the crystallizer is 3800L / min; Water distribution in the secondary cooling section: The cooling water volume of the full roll section is 80L / min, the cooling water volume of the vertical section is 60L / min, the water volume of the outer arc of the bending section is 45L / min, and the inner arc is 30L / min; The cooling water volume of the straightening section is 75L / min for the outer arc, and 45L / min for the inner arc, so that the solidification end is located between 18.50m from the liquid surface of the crystallizer; The continuous casting crystallizer protective slag adopts the existing protective slag for bridge steel, and the thickness of the liquid slag layer is controlled to be in the range of 6mm, the basicity of the liquid slag is in the range of 0.65mm, and the viscosity is in the range of 0.43Pa·s.
[0022] Take the obtained ingot sample for analysis: Figure 1 As shown in the figure, the billet has no obvious looseness or shrinkage (the looseness or shrinkage level of the billet is ≤0.5), and there is no edge crack at the corner. However, the existing continuous casting billet for bridge steel has problems such as looseness in the center, easy corner defects, and excessive large inclusions in the billet (such as Figure 2 shown).
[0023] Example 2
[0024] 1) Smelting and continuous casting: conventional smelting, control the temperature of the upper continuous casting platform, during continuous casting, control the temperature of the tundish to be 17°C higher than the liquidus (liquidus temperature is 1511-1524°C), the pulling speed is controlled at 0.85m / min, dynamic soft pressure is adopted at the end of solidification and electromagnetic stirring technology is used to continuously cast into 230*2150mm slabs, among which the liquid core is pressed down by 7mm, the electromagnetic stirring current is 450A, and the frequency is 6HZ; the tundish is controlled by full package, and the control At around 40 tons, the middle package is equipped with a slag retaining wall and a slag retaining dam. The middle wall height of the slag retaining wall is 1025mm, the upper width is 1950mm, the lower width is 1590mm, and there are two square holes in a single row. The size of the square holes is 120*120mm, and the outer side is inclined 12° in the horizontal direction. Two circular holes with a diameter of 80mm are opened on each side wall; the slag retaining dam is 300mm high and forms an angle of 77° to the slag retaining wall. The double drainage outlets are symmetrically distributed, and the water inlet insertion depth is 135mm.
[0025] 2) Cooling water configuration: The water volume of the crystallizer is 4200L / min. Water distribution in the second cooling section: 140L / min of cooling water for the full roll section, 80L / min of cooling water for the vertical section, 50L / min of cooling water for the outer arc of the bending section, and 35L / min of cooling water for the inner arc; 77L / min of cooling water for the outer arc of the straightening section, and 47L / min of cooling water for the inner arc. This makes the solidification end located between 19.0m and the crystallizer liquid surface; the continuous casting crystallizer protective slag adopts the existing protective slag for bridge steel, and the liquid slag layer thickness is controlled within the range of 7mm, the liquid slag alkalinity is within the range of 0.66mm, and the viscosity is within the range of 0.44Pa·s.
[0026] The obtained ingot samples were taken for analysis: the ingot had no obvious porosity or shrinkage (the porosity or shrinkage level of the ingot was ≤0.5), and there was no edge crack at the corners.
[0027] Example 3
[0028] 1) Smelting and continuous casting: For conventional smelting, the temperature of the upper continuous casting platform is controlled. During continuous casting, the temperature of the middle package is controlled to be 20°C higher than the liquidus (the liquidus temperature is 1511-1524°C), the pulling speed is controlled at 0.89m / min, and the dynamic soft pressure at the end of solidification is adopted in combination with electromagnetic stirring technology to continuously cast into 230*2150mm slabs, wherein the liquid core is pressed down by 9mm, the electromagnetic stirring current is 450A, and the frequency is 6HZ; the middle package is controlled by full package and controlled at about 40 tons. The middle package is equipped with a retaining wall and a slag dam. The height of the middle wall of the retaining wall is 1030mm, the width of the upper mouth is 2000mm, the width of the lower mouth is 1600mm, and there are two square holes in a single row. The size of the square hole is 120*120mm, the outer side is inclined by 15° in the horizontal direction, and two circular holes with a diameter of 80 are opened on each side wall; the slag dam is 350mm high, forming an 80° angle to the slag retaining wall, the double drainage outlets are symmetrically distributed, and the water nozzle insertion depth is 155mm.
[0029] 2) Cooling water configuration: The water volume of the crystallizer is 4800L / min. Water distribution in the second cooling section: 230L / min of cooling water for the full roll section, 120L / min of cooling water for the vertical section, 55L / min of cooling water for the outer arc of the bending section, and 40L / min of cooling water for the inner arc; 80L / min of cooling water for the outer arc of the straightening section, and 50L / min of cooling water for the inner arc. This makes the solidification end located 19.40m away from the liquid surface of the crystallizer; the protective slag of the continuous casting crystallizer adopts the existing protective slag for bridge steel, and the thickness of the liquid slag layer is controlled to be 9mm, the basicity of the liquid slag is 0.67mm, and the viscosity is 0.45Pa·s.
[0030] The obtained ingot samples were taken for analysis: the ingot had no obvious porosity or shrinkage (the porosity or shrinkage level of the ingot was ≤0.5), and there was no edge crack at the corners.
Claims
1. A method for improving the quality of bridge steel ingots, comprising smelting, continuous casting and cooling steps, characterized in that: In the continuous casting step, the temperature of the tundish is controlled to be 15-20°C higher than the liquidus line, and the pulling speed is controlled to be 0.8-0.9 m / min; in the cooling step, the water distribution in the second cooling section is as follows: the cooling water volume of the foot roll section is 80-230 L / min, the cooling water volume of the vertical section is 60-120 L / min, the water volume of the outer arc of the bending section is 45-55 L / min, the water volume of the inner arc of the bending section is 30-40 L / min, the cooling water volume of the outer arc of the straightening section is 75-80 L / min, and the cooling water volume of the inner arc of the straightening section is 45-50 L / min; In the continuous casting step, the middle ladle is controlled to be full at 35 to 45 tons, and a slag retaining wall and a slag retaining dam are arranged in the middle ladle. The middle wall height of the slag retaining wall is 1020 to 1030 mm, the upper width is 1900 to 2000 mm, the lower width is 1580 to 1600 mm, and the outer side inclination is 10 to 15° in the horizontal direction; the slag retaining dam is 250 to 350 mm high, forming an angle of 75 to 80° with the slag retaining wall, and the double drainage outlets are symmetrically distributed, and the water inlet insertion depth is 120 to 160 mm.
2. The method for improving the quality of bridge steel casting according to claim 1, characterized in that: In the continuous casting step, the solidification end is subjected to liquid core pressing process and electromagnetic stirring to continuously cast into a slab.
3. The method for improving the quality of bridge steel casting according to claim 2, characterized in that: In the continuous casting step, the liquid core is pressed down by 5 to 10 mm, the electromagnetic stirring current is 440 to 460 A, and the frequency is 5 to 8 Hz.
4. The method for improving the quality of bridge steel casting according to claim 1, characterized in that: The slag retaining wall of the middle bag is provided with two square holes in a single row, and two round holes are respectively opened on the two side walls of the middle bag.
5. The method for improving the quality of bridge steel casting according to claim 1, characterized in that: In the cooling step, the solidification end is 18.50 to 19.50 m away from the liquid surface of the crystallizer.
6. The method for improving the quality of bridge steel casting according to claim 1, characterized in that: In the continuous casting step, the thickness of the liquid slag layer of the continuous casting mold protection slag is controlled to be 6-10 mm, the basicity of the liquid slag is controlled to be 0.65-0.68 mm, and the viscosity is controlled to be 0.43-0.46 Pa·s.