Method for depositing group IV semiconductor and related semiconductor device structure
By using group IIIA dopant precursors such as borohydride for chemical vapor deposition on the surface of group IV semiconductors, the problems of increasing carrier density and maintaining crystal quality in p-type MOS devices are solved, achieving low contact resistivity and Effect of high carrier mobility.
Patent Information
- Application Number
- CN201810594778.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-07-19
- Filing Date
- 2018-06-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-04-10
AI Technical Summary
When the existing technology increases the carrier density of the doped stress source region in p-type MOS devices, it easily leads to a decrease in crystal quality, and it is difficult to reduce the contact resistivity.
Achieve high p-type carrier density and maintain crystallinity by depositing Group IIIA dopant precursors containing borohydrides, organoboronhydrides, halides or organic halides on the Group IV semiconductor surface via chemical vapor deposition. quality.
It achieves the improvement of high p-type doping density in Group IV semiconductors, while reducing the contact resistivity of semiconductor devices and improving carrier mobility and device performance.
Smart Images

Figure HDA0001691213830000011 
Figure HDA0001691213830000021
Abstract
Description
[0001] Cross-references to related patent applications
[0002] This disclosure claims the benefit of U.S. Provisional Patent Application No. 62 / 534,618, filed on July 19, 2017, and entitled “A METHOD FOR DEPOSITING A GROUP IV SEMICONDUCTOR AND RELATED SEMICONDUCTOR DEVIC E STRUCTURES,” which is incorporated herein by reference. Technical Field
[0003] The present disclosure generally relates to methods of depositing Group IV semiconductors and related semiconductor device structures. The present disclosure also generally relates to methods of doping Group IV semiconductors and doping precursors that can be used for p-type doping of Group IV semiconductors. Background Art
[0004] The miniaturization of semiconductor device structures such as complementary metal oxide semiconductor (CMOS) devices has brought about significant improvements in the speed and density of integrated circuits. However, conventional device miniaturization faces great challenges in future technology nodes.
[0005] One approach to improving semiconductor device performance is to utilize strain-induced effects to increase carrier mobility and, therefore, transistor drive current. For example, it has been shown that hole mobility can be significantly increased in p-channel silicon (Si) transistors that employ stressor regions, such as those employed in the source and drain regions of a transistor structure.
[0006] The contact resistance to the active region of a semiconductor device structure may be a concern for ongoing device improvements at future technology nodes. For example, for a CMOS device structure, the contact resistance may include the resistance between the contact structure and one or more stressor regions including the source and drain regions of the transistor structure. For an n-type MOS device, the stressor region may include a highly doped region doped with phosphorus or arsenic, i.e., with a resistance of approximately 5×10 20 cm -3 的载流子密度 The high doping levels achievable in stressor regions of n-type MOS devices can result in contact resistivities as low as 0.3 mΩ-cm. However, for p-type MOS devices, prior art has focused on the use of boron p-type doping using boron dopant precursors such as diborane (B2H6). The use of diborane (B2H6) in p-type MOS devices can result in contact resistivities of approximately 1×10 20 cm -3Efforts to increase the p-type carrier density in p-type MOS devices by adding additional boron may result in a degradation of the crystalline quality of the doped stressor region and may not contribute significantly to the active carrier density in the p-type stressor region. Therefore, there is a need for alternative methods and precursors that can achieve high p-type doping density in semiconductor materials such as Group IV semiconductor materials. Summary of the invention
[0007] According to at least one embodiment of the present disclosure, a method for depositing a Group IV semiconductor on the surface of a semiconductor is disclosed. The method may include providing a substrate in a reaction chamber, heating the substrate to a deposition temperature, exposing the substrate to at least one Group IV precursor, and exposing the substrate to at least one Group IIIA dopant precursor, wherein the at least one Group IIIA dopant precursor comprises a borohydride, an organic borohydride, a halide, or an organic halide. Embodiments of the present disclosure may also include a semiconductor device structure, which may include a Group IV semiconductor deposited by the method of the present disclosure.
[0008] In order to summarize the present invention and the advantages achieved over the prior art, certain objects and advantages of the present invention have been described above. Of course, it should be understood that not all of these objects or advantages may be achieved according to any particular embodiment of the present invention. Thus, for example, it should be appreciated by those skilled in the art that the present invention may be implemented or performed in a manner that achieves or optimizes one advantage or a group of advantages as taught or suggested herein without necessarily achieving other objects or advantages as may be taught or suggested herein.
[0009] All these embodiments are intended to be included within the scope of the disclosed invention. These and other embodiments will be apparent to those skilled in the art through the following detailed description of certain embodiments in conjunction with the accompanying drawings, and the present invention is not limited to any particular embodiment disclosed. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Although this specification ends with claims that specifically point out and distinctly claim to be considered part of embodiments of the present invention, advantages of the embodiments of the present disclosure may be more readily ascertained from the description of certain examples of the embodiments of the present disclosure when read in conjunction with the accompanying drawings, in which:
[0011] Figure 1 illustrates a process flow diagram illustrating an exemplary deposition method according to an embodiment of the present disclosure; and
[0012] Figure 2 A schematic diagram of a semiconductor device structure including a p-type doped Group IV semiconductor deposited according to an embodiment of the present disclosure is illustrated.
[0013] It should be understood that the elements in the figures are illustrated for simplicity and clarity only and are not necessarily drawn to scale. For example, the dimensions of some elements in the figures may be exaggerated relative to other elements to help improve understanding of the embodiments of the present disclosure illustrated. DETAILED DESCRIPTION
[0014] Although certain embodiments and examples are disclosed below, it will be appreciated by those skilled in the art that the present invention extends beyond the specifically disclosed embodiments and / or uses of the present invention and obvious modifications and equivalents thereof. Therefore, it is contemplated that the scope of the present invention disclosed should not be limited by the specific disclosed embodiments described below.
[0015] As used herein, the term "substrate" may refer to any underlying material or materials that may be used or upon which a device, circuit, or film may be formed.
[0016] As used herein, the term “Group IV semiconductor” may refer to a semiconductor material including at least one of carbon (C), silicon (Si), germanium (Ge), tin (Sn), or an alloy thereof.
[0017] As used herein, the term “Group IIIA dopant precursor” may refer to a dopant precursor including at least one of boron (B), aluminum (Al), gallium (Ga), or indium (In).
[0018] Embodiments of the present disclosure may include methods for depositing a Group IV semiconductor, and in particular, methods for depositing a Group IV semiconductor containing a Group IIIA dopant. As a non-limiting example of an embodiment of the present disclosure, the method may include depositing a Group IV semiconductor layer containing a Group IIIA dopant, such as a dopant containing at least one of boron (B), aluminum (Al), gallium (Ga), or indium (In). The methods of the present disclosure utilize novel Group IIIA dopant precursors that can achieve high active carrier concentrations, such as up to greater than about 1×10 20 cm -3 的有源载流子浓度. The method of the present disclosure may also utilize novel Group IIIA dopant precursors to achieve high active p-type carrier concentrations in Group IV semiconductors, the novel Group IIIA dopant precursors comprising one or more of Group IIIA dopant precursors such as borohydrides, organic borohydrides, halides, or organic halides. The novel Group IIIA dopant precursors described herein for achieving high active p-type carrier concentrations in Group IV semiconductors may not only provide high carrier concentrations, but also maintain the crystalline quality of the Group IV semiconductor. For example, Group IV semiconductors are most commonly doped with boron using diborane (B2H6). However, adding boron to stressor regions, such as adding boron to silicon germanium stressor regions, may reduce the total strain applied by the stressor regions, resulting in a reduction in carrier mobility and thereby reducing semiconductor device performance. The novel Group IIIA dopants described herein also allow for a reduction in electrical contact resistance with semiconductor device structures such as transistor structures.
[0019] Can be combined Figure 1 To understand the method of the present disclosure, the figure illustrates a non-limiting example embodiment of a method for forming a Group IV semiconductor. For example, Figure 1 A method 100 for forming a Group IV semiconductor may be illustrated, which may include a process module 110, wherein a substrate may be provided to a reaction chamber and may be heated to a deposition temperature within the reaction chamber. As a non-limiting example, the reaction chamber may include a reaction chamber of a chemical vapor deposition system. Embodiments of the present disclosure may be referred to as Intrepi d TM XP or The present disclosure is performed in a chemical vapor deposition system obtained from ASM International NV. However, it is also contemplated that other reaction chambers, such as atomic layer deposition reaction chambers and alternative chemical vapor deposition systems from other manufacturers may be employed to perform embodiments of the present disclosure.
[0020] In some embodiments of the present disclosure, the substrate may include a planar substrate or a patterned substrate. The patterned substrate may include a substrate that may include a semiconductor device structure formed in the substrate or on the substrate surface, for example, the patterned substrate may include a partially manufactured semiconductor device structure such as a transistor and a memory element. The substrate may contain a single crystal surface and / or one or more sub-surfaces, and the sub-surface may include a non-single crystal surface, such as a polycrystalline surface and an amorphous surface. The single crystal surface may include, for example, one or more of the following: silicon (Si), silicon germanium (SiGe), germanium tin (GeSn) or germanium (Ge). The polycrystalline or amorphous surface may include a dielectric material, such as an oxide, an oxynitride or a nitride, including, for example, silicon oxide and silicon nitride.
[0021] Continue to refer Figure 1, method 100 may continue by heating the substrate within the reaction chamber to a desired deposition temperature. In some embodiments of the present disclosure, method 100 may include heating the substrate to a temperature below about 700° C., or to a temperature below about 600° C., or to a temperature below about 500° C., or to a temperature below about 400° C., or even to a temperature below about 300° C. For example, in some embodiments of the present disclosure, heating the substrate to the deposition temperature may include heating the substrate to a temperature between about 280° C. and about 700° C.
[0022] After the substrate is heated to the desired deposition temperature, method 100 may continue by exposing the substrate to one or more deposition precursors, which may include one or more precursors for depositing the Group IV semiconductor and may also include one or more precursors for doping the Group IV semiconductor with one or more p-type dopants.
[0023] Thus, the methods of the present disclosure may include exposing a substrate to at least one Group IV precursor, such as Figure 1 In some embodiments, exposing the substrate to at least one Group IV precursor may further include selecting the at least one Group IV precursor to be one of the following: monosilane (SiH4), disilane (Si2H6), trisilane (Si3H8), tetrasilane (Si4H 10 ), isopentasilane (Si5H 12 ), neopentasilane (Si5H 12 ), dichlorosilane (DCS), germane (GeH4), digermane (Ge2H6), propigermane (Ge3H8), germanylsilane (GeH6Si), tin tetrachloride (SnCl4) or methylsilane (CH3-SiH3).
[0024] In some embodiments, a single Group IV precursor may be used during the deposition process, for example, when the Group IV semiconductor to be deposited comprises silicon (Si) or germanium (Ge), a single Group IV precursor may be used. In some embodiments, two or more Group IV precursors may be used during the deposition process, for example, when the Group IV semiconductor to be deposited comprises a Group IV semiconductor alloy, two or more Group IV precursors may be used, including but not limited to silicon germanium carbide (Si 1-x-y Ge x C y ), Germanium Tin (Ge 1-x Sn x )、GeSiSn 1-x-y Si x Sn y ), Germanium Silicon Tin Carbide (Ge 1-x-y Si x Sn y C x )、Silicon Tin (Si1-x Sn x ), Silicon Tin Carbide (Si 1-x- y Sn x C y ) or silicon carbide (Si 1-x C x ).
[0025] The deposition process for depositing a Group IV semiconductor may also include exposing the substrate to at least one Group IIIA dopant precursor. For example, in some embodiments of the present disclosure, Figure 1 The deposition method 100 illustrated in the accompanying drawings may include exposing a substrate to at least one Group IV precursor and also exposing the substrate to at least one Group IIIA dopant precursor, i.e., the Group IV precursor and the Group IIIA dopant precursor are co-flowed into a reaction chamber and react / decompose on a surface of a substrate disposed in the reaction chamber. The co-flow of the one or more Group IV precursors and the one or more Group IIIA dopant precursors into the reaction chamber may be utilized to allow dopant species to be introduced into the Group IV semiconductor along with the deposition of the Group IV semiconductor.
[0026] In some embodiments, exposing the substrate to at least one Group IIIA dopant precursor may include exposing the substrate to at least one of a borohydride, an organoborohydride, a halide, or an organohalide.
[0027] In some embodiments of the present disclosure, exposing the substrate to at least one Group IIIA dopant precursor may include exposing the substrate to at least one or more borohydrides, including gallium borohydride (Ga(BH4)3), aluminum borohydride (Al(BH4)3), or indium borohydride (In(BH4)3). In alternative embodiments of the present disclosure, exposing the substrate to at least one Group IIIA dopant precursor may include selecting the borohydride to include a borohydride having the formula Y x M(BH4) 3-x A borohydride of , wherein Y is independently selected from hydrogen, deuterium, chlorine, bromine and iodine; M is a Group IIIA metal independently selected from gallium, aluminum and indium; and x is an integer of 0-2.
[0028] In some embodiments of the present disclosure, exposing the substrate to at least one Group IIIA dopant precursor may include exposing the substrate to one or more dopants having the general formula R x M(BH4) 3-x An organic borohydride, wherein R is independently selected from CH3, C2H5, C6H5, CF3SO3 and NH2; M is a Group IIIA metal independently selected from gallium, aluminum and indium; and x is an integer of 1-3.
[0029] In some embodiments of the present disclosure, exposing the substrate to at least one Group IIIA dopant precursor may include exposing the substrate to one or more dopants having the general formula Zx MY 3-x wherein Z is independently selected from hydrogen, deuterium, chlorine, bromine and iodine; M is a Group IIIA metal independently selected from gallium, aluminum and indium; Y is a halide independently selected from chlorine, bromine and iodine; and x is an integer from 0 to 3. In some embodiments of the present disclosure, the halide dopant may include a dimer structure, and thus the method may include selecting a halide to include a halide having the formula (Z x MY 3-x )2 halide, wherein Z is independently selected from hydrogen, deuterium, chlorine, bromine and iodine; M is a Group IIIA metal independently selected from gallium, aluminum and indium; Y is a halide independently selected from chlorine, bromine and iodine; and x is an integer from 0 to 3.
[0030] In some embodiments of the present disclosure, exposing the substrate to at least one Group IIIA dopant precursor may include selecting the Group IIIA dopant to include one or more organic halides and may further include selecting the one or more organic halides to include a compound having the general formula R x MY 3-x An organic halide, wherein R is independently selected from CH3, C2H5, C6H5, CF3SO3 and NH2; M is a Group IIIA metal independently selected from gallium, aluminum and indium; Y is a halide independently selected from chlorine, bromine and iodine; and x is an integer of 0-3.
[0031] Selecting a Group IIIA dopant precursor comprising an organic component may be further beneficial in the deposition of a Group IV semiconductor. For example, the introduction of carbon into a Group IV semiconductor may further increase the strain in the Group IV semiconductor being deposited. Therefore, in some embodiments of the present disclosure, exposing the substrate to at least one Group IIIA precursor further comprises exposing the substrate to at least one of an organic borohydride or an organic halide. In other embodiments, exposing the substrate to at least one of an organic borohydride or an organic halide further comprises introducing carbon into the deposited Group IV semiconductor, the atomic percentage (at-%) of carbon in the Group IV semiconductor being greater than about 0.5% at-%.
[0032] In some embodiments of the present disclosure, two or more dopant species may be introduced into the deposited Group IV semiconductor. For example, in some embodiments, exposing the substrate to at least one Group IIIA dopant precursor further comprises exposing the substrate to at least one of a borohydride or an organic borohydride. In embodiments employing a borohydride or an organic borohydride, the dopant precursor contains boron (B) in addition to another Group IIIA dopant (e.g., gallium, aluminum, or indium). Thus, employing a borohydride or an organic borohydride comprises introducing a boron dopant and another Group III A dopant into the deposited Group IV semiconductor. Such methods may be employed to further increase the dopant concentration in the Group IV semiconductor without a corresponding reduction in the crystalline quality of the Group IV semiconductor.
[0033] Embodiments of the present disclosure may Figure 1 The process module 140 continues with the step of depositing a Group IV semiconductor on a surface of a substrate disposed in a reaction chamber. In some embodiments, depositing a Group IV semiconductor on the surface of the substrate includes depositing silicon (Si), germanium (Ge), silicon germanium (Si 1-x Ge x ), Silicon Germanium Carbide (Si 1-x-y Ge x C y ), Germanium Tin (Ge 1-x Sn x )、GeSiSn 1-x- y Si x Sn y ), Germanium Silicon Tin Carbide (Ge 1-x-y Si x Sn y C x )、Silicon Tin (Si 1-x Sn x ), Silicon Tin Carbide (Si 1-x-y Sn x C y ) or silicon carbide (Si 1-x C x )
[0034] The methods of the present disclosure allow for the deposition of Group IV semiconductors with high p-type dopant concentrations without reducing the crystalline quality of the Group IV semiconductor. For example, in some embodiments, depositing the Group IV semiconductor on the surface of the substrate further comprises depositing the Group IV semiconductor at a concentration greater than about 1×10 20 carriers per cubic centimeter, or greater than about 2.5×10 20 carriers per cubic centimeter, or even greater than about 5×10 20 Group IV semiconductors are deposited with a doping concentration of carriers per cubic centimeter.
[0035] Embodiments of the present disclosure may also provide semiconductor device structures comprising a Group IV semiconductor deposited by the methods described herein. For example, Figure 2 A non-limiting example of a semiconductor device structure 200 is illustrated, wherein the semiconductor device structure 200 includes a dual-gate MOSFET, commonly referred to as a FinFET. The semiconductor device structure 200 may include a substrate 202, which may include a bulk silicon (Si) substrate. The substrate 202 may be doped with a p-type dopant (for an NMOS type FinFET device) or doped with an n-type dopant (for a PMOS type FinFET device). Figure 2In a non-limiting example of a semiconductor device structure of FIG. 1 , the substrate 200 may include an n-type dopant and the semiconductor device structure 200 may include a P MOS FinFET.
[0036] The semiconductor device structure 200 may also include an isolation region 204, which may include a shallow trench isolation (STI) region. The semiconductor device structure 200 may also include a fin structure 206 extending above the top surface of the isolation region 204. A gate dielectric (not shown) may be disposed over the sidewalls of the fin structure 206, and the gate dielectric may include silicon oxide or a high-k dielectric material. A gate electrode 208 may be disposed on the gate dielectric to provide electrical contact with a channel region within the fin structure 206. The semiconductor device structure 200 may also include a gate spacer 210 disposed on the sidewalls of the gate electrode 208.
[0037] In some embodiments of the present disclosure, the semiconductor device structure 200 may further include p-type Group IV semiconductor stressor regions 212A and 212B deposited over the source and drain regions of the FinFET device. It should be noted that the p-type stressor regions 212A and 212B may include multiple facets that may result from differences in growth rates on different facets of the fin structure 206. In a non-limiting example embodiment of the present disclosure, the p-type stressor regions 212A and 212B may be deposited using the embodiments of the present disclosure described herein. For example, the p-type stressor regions 212A and 212B may include silicon germanium (Si 1-x Ge x ), wherein the germanium content in the silicon germanium stressor region may be greater than about x>0.2, or greater than about x>0.50, or greater than about x>0.75, or even about x=1.0. In addition, the p-type stressor regions 212A and 212B may be doped according to embodiments of the present disclosure and thus the p-type stressor regions 212A and 212B may contain greater than about 1×10 20 carriers per cubic centimeter, or greater than about 2.5×10 20 carriers per cubic centimeter, or even about 5×10 20 The p-type doping concentration is carriers per cubic centimeter.
[0038] In some embodiments of the present disclosure, the Figure 2The disclosed embodiments provide electrical contacts to p-type Group IV semiconductor stressor regions 212A and 212B above the source and drain regions of the FinFET device illustrated in FIG. 1 . In some embodiments, the electrical contacts (not shown) may include a silicide such as titanium silicide (TiSi2). Embodiments of the present disclosure allow for high active p-type carrier concentrations in the source and drain stressor regions 212A and 212B, which in turn may result in reduced electrical contact resistance to the stressor regions. For example, the disclosed methods may include forming electrical contacts to the p-type stressor regions 212A and 212B, wherein the electrical contacts have a resistance of less than 1×10 -9 Ohm.cm 2 , or less than 5×10 -9 Ohm.cm 2 , or even less than 1×10 -8 Ohm.cm 2 Resistivity.
[0039] It should be noted that one non-limiting example embodiment presented herein relates to p-type stressor regions formed over source and drain regions of a FinFET device. However, embodiments of the present disclosure may be used for other purposes, for example, p-type Group IV semiconductors deposited by embodiments of the present disclosure may be employed to induce stress in other regions of a device structure, such as by depositing a p-type stressor region over a channel region of a transistor to thereby induce strain directly in the channel region of a transistor device structure.
[0040] The example embodiments of the present disclosure described above do not limit the scope of the present invention, because these embodiments are only examples of embodiments of the present invention, and the present invention is limited by the attached claims and their legal equivalents. Any equivalent embodiments are intended to be included in the scope of the present invention. In fact, various modifications of the present disclosure, such as the alternative available combinations of the elements, in addition to those shown and described herein, will be apparent to those skilled in the art from the specification. Such modifications and embodiments are also intended to fall within the scope of the attached claims.
Claims
1. A method for depositing a Group IV semiconductor on a surface of a substrate, the method comprising: include: providing a substrate within a reaction chamber; heating the substrate to a deposition temperature below 500° C.; exposing the substrate to at least one Group IV precursor; and Exposing the substrate to at least one Group IIIA dopant precursor, wherein the at least one Group IIIA dopant precursor comprises: at least one of a borohydride and an organic borohydride, wherein the borohydride has a general formula Y x M(BH 4 ) 3-x , wherein Y is independently selected from hydrogen, deuterium, chlorine, bromine and iodine; M is a Group IIIA metal independently selected from gallium, aluminum and indium; and x is an integer of 0-2.
2. The method of claim 1, wherein the at least one Group IIIA dopant precursor comprises a borohydride selected from the group consisting of gallium borohydride (Ga(BH 4 ) 3 )、Aluminum borohydride(Al(BH 4 ) 3 ) or indium borohydride (In(BH 4 ) 3 ).
3. The method of claim 1, wherein the at least one Group IIIA dopant precursor comprises a precursor having the formula R x M(BH 4 ) 3-x An organic borohydride, wherein R is independently selected from CH 3 , C 2 H 5 , C 6 H 5 CF 3 SO 3 and NH 2 ; M is a Group IIIA metal independently selected from gallium, aluminum and indium; x is an integer of 1-3.
4. The method of claim 1, wherein exposing the substrate to at least one Group IV precursor further comprises selecting the at least one Group IV precursor to include monosilane (SiH 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), butadienesilane (Si 4 H 10 ), isopentasilane (Si 5 H 12 ), neopentasilane (Si 5 H 12 ), dichlorosilane (DCS), germanium (GeH 4 ), Digermane (Ge 2 H 6 ), propiogermane (Ge 3 H 8 ), germanylsilane (GeH 6 Si), tin tetrachloride (SnCl 4 ) or methylsilane (CH 3 -SiH 3 ).
5. The method of claim 1, wherein depositing a Group IV semiconductor on the surface of the substrate further comprises depositing at least one of the following: silicon (Si), germanium (Ge), silicon germanium (Si 1-x Ge x )、Silicon Germanium Carbide(Si 1-x-y Ge x C y )、Ge 1- x Sn x )、Ge-Si-Sn(Ge 1-x-y Si x Sn y )、Ge-Si-Tn Carbide(Ge 1-x-y Si x Sn y C x )、Silicon Tin(Si 1-x Sn x )、Silicon Tin Carbide(Si 1-x-y Sn x C y ) or silicon carbide (Si 1-x C x ).
6. The method of claim 1, wherein depositing a Group IV semiconductor on the surface of the substrate further comprises depositing a Group IV semiconductor on the surface of the substrate at a depth greater than 1×10 20 The Group IV semiconductor is deposited with a doping concentration of carriers per cubic centimeter.
7. The method of claim 1, wherein exposing the substrate to at least one Group IIIA dopant precursor further comprises exposing the substrate to at least one of an organic borohydride or an organic halide.
8. The method of claim 7, wherein exposing the substrate to at least one of an organic borohydride or an organic halide further comprises introducing carbon into the deposited Group IV semiconductor, the atomic percentage of carbon in the Group IV semiconductor being greater than 0.5 at-%.
9. The method of claim 1, wherein exposing the substrate to at least one Group IIIA dopant precursor further comprises exposing the substrate to at least one of a borohydride or an organoborohydride.
10. The method of claim 9, wherein exposing the substrate to at least one of a borohydride or an organic borohydride further comprises introducing a boron dopant and an additional Group IIIA dopant into the deposited Group IV semiconductor.
11. A semiconductor device structure comprising a Group IV semiconductor deposited according to the method of claim 1. 12 . The semiconductor device structure of claim 11 , wherein the Group IV semiconductor comprises a p-type stressor region.
13. The semiconductor device structure of claim 12, further comprising forming an electrical contact with the p-type stressor region, wherein the electrical contact has a thickness less than 1×10 -8 Ohm.cm 2 Resistivity.