Thermoplastic resin composition and laminate using the same

By using cyclic polyolefin polymers, aromatic vinyl compounds and conjugated diene compounds in the thermoplastic resin composition, the problem of insufficient adhesion between the cyclic polyolefin polymer and the metal is solved, and high strength and high strength are achieved Preparation of impact-resistant laminated body.

CN109642070BActive Publication Date: 2024-11-19RIKEN TECHNOS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201780051648.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-08-31
Filing Date
2017-08-25
Publication Date
2024-11-19
Estimated Expiration
2037-08-25

AI Technical Summary

Technical Problem

The adhesion of existing cyclic polyolefin polymers and metals such as ethylene-vinyl alcohol copolymers or aluminum foils is insufficient, resulting in insufficient bonding strength.

Method used

Adhesive coatings or laminates are prepared by melt-kneading process using a thermoplastic resin composition containing a copolymer of a cyclic polyolefin polymer, an aromatic vinyl compound and a conjugated diene compound, or a hydrogenation product thereof, and the adhesive coating or laminate is prepared by a melt-kneading process. to improve bond strength.

Benefits of technology

Full bonding of the cyclic polyolefin polymer with ethylene-vinyl alcohol copolymer or aluminum foil is achieved, which improves the bonding strength and impact resistance, while maintaining the characteristics of the raw material and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0001975732320000211
    Figure BDA0001975732320000211
  • Figure BDA0001975732320000212
    Figure BDA0001975732320000212
  • Figure BDA0001975732320000221
    Figure BDA0001975732320000221
Patent Text Reader

Abstract

The present invention provides a thermoplastic resin composition capable of bonding a cyclic polyolefin polymer and an ethylene-vinyl alcohol copolymer or a metal foil with sufficient strength, and a laminate using the same. The present invention provides a thermoplastic resin composition comprising: (A) 100 parts by mass of a thermoplastic resin; (B) 0.05 to 5 parts by mass of at least one selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids; and (C) 0.01 to 3 parts by mass of an organic peroxide, wherein the thermoplastic resin (A) comprises: (a1) 10 to 90% by mass of a cyclic polyolefin polymer; and (a2) 90 to 10% by mass of at least one selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof; the total of the components (a1) and (a2) is 100% by mass, and the component (a2) excludes hydrogenated products of block copolymers consisting of polymer blocks mainly composed of aromatic vinyl compounds and random copolymer blocks of conjugated diene compounds and aromatic vinyl compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoplastic resin composition, and more particularly to a thermoplastic resin composition containing a cyclic polyolefin polymer, a copolymer of an aromatic vinyl compound and a conjugated diene compound and / or a hydrogenated product thereof, and a laminate using the composition. Background Art

[0002] At present, the laminate of cyclic polyolefin polymer and ethylene-vinyl alcohol copolymer has excellent strength, transparency, gas barrier and chemical resistance, and therefore is used as packaging film or container. In addition, as a packaging film or container for packaging contents that are very weak to oxygen or moisture, the laminate of cyclic polyolefin polymer and metal or metal compound such as aluminum foil has very high gas barrier, strength and chemical resistance, and is therefore used. However, there is a problem of insufficient adhesion between cyclic olefin polymer and metal or metal compound such as ethylene-vinyl alcohol copolymer or aluminum foil. Therefore, it is proposed to use polyolefin polymer or its acid modified substance as an adhesive component so that it is between the two (for example, patent documents 1, 2). However, with regard to these technologies, the bonding strength is not sufficient, and it is desired to improve the bonding strength.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 11-070624

[0006] Patent Document 2: Japanese Patent Application Publication No. 2003-191380 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] One object of the present invention is to provide a thermoplastic resin composition capable of bonding a cyclic polyolefin polymer and an ethylene-vinyl alcohol copolymer with sufficient strength, and a laminate using the same. Another object of the present invention is to provide a thermoplastic resin composition capable of bonding a cyclic polyolefin polymer and a metal or a metal compound such as an aluminum foil with sufficient strength, and a laminate using the same.

[0009] Technical solutions to solve problems

[0010] As a result of intensive studies, the present inventors have found that a specific thermoplastic resin composition can achieve the above-mentioned objects.

[0011] That is, the first present invention is a thermoplastic resin composition comprising:

[0012] (A) 100 parts by mass of a thermoplastic resin,

[0013] (B) 0.05 to 5 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids, and

[0014] (C) 0.01 to 3 parts by mass of an organic peroxide,

[0015] The (A) thermoplastic resin comprises:

[0016] (a1) 10 to 90% by mass of a cyclic polyolefin polymer, and

[0017] (a2) 90 to 10% by mass of one or more selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof,

[0018] Here, the total amount of the component (a1) and the component (a2) is 100% by mass.

[0019] The component (a2) excludes hydrogenated products of block copolymers composed of a polymer block mainly composed of an aromatic vinyl compound and a random copolymer block of a conjugated diene compound and an aromatic vinyl compound.

[0020] The second invention is the thermoplastic resin composition according to the first invention, wherein the component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms.

[0021] The third invention is the thermoplastic resin composition according to the first invention or the second invention, wherein the component (a2) is a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

[0022] The fourth invention is the thermoplastic resin composition according to the first invention or the second invention, wherein the component (a2) is a hydrogenated product of a random copolymer of an aromatic vinyl compound and a conjugated diene compound.

[0023] A fifth invention is an adhesive coating material comprising the thermoplastic resin composition according to any one of the first to fourth inventions.

[0024] The sixth invention is the coating material according to the fifth invention, wherein the component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms.

[0025] The seventh invention is a laminated body obtained by laminating a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to any one of the first to fourth inventions, and a layer composed of a resin having a polar group in this order.

[0026] The eighth invention is a laminated body, which is obtained by laminating in order a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition described in any one of the first to fourth inventions, a layer composed of a resin having a polar group, a layer composed of the thermoplastic resin composition described in any one of the first to fourth inventions, and a layer composed of a cyclic polyolefin polymer.

[0027] The ninth invention is the laminate according to the seventh invention or the eighth invention, wherein the resin having a polar group is an ethylene-vinyl alcohol copolymer.

[0028] The tenth invention is a laminated body obtained by laminating a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to any one of the first to fourth inventions, and a layer composed of a metal or a metal compound in this order.

[0029] The eleventh invention is a laminated body obtained by laminating in this order a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to any one of the first to fourth inventions, a layer composed of a metal or a metal compound, a layer composed of the thermoplastic resin composition according to any one of the first to fourth inventions, and a layer composed of a cyclic polyolefin polymer.

[0030] The twelfth invention is the laminate according to the tenth invention or the eleventh invention, wherein the layer composed of the metal or the metal compound is a layer composed of aluminum foil.

[0031] The 13th invention is a method for producing a thermoplastic resin composition, comprising the step of melt-kneading a thermoplastic resin composition, wherein the composition comprises:

[0032] (A) 100 parts by mass of a thermoplastic resin,

[0033] (B) 0.05 to 5 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids, and

[0034] (C) 0.01 to 3 parts by mass of an organic peroxide,

[0035] The (A) thermoplastic resin comprises:

[0036] (a1) 10 to 90% by mass of a cyclic polyolefin polymer, and

[0037] (a2) 90 to 10% by mass of one or more selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof,

[0038] Here, the total amount of the component (a1) and the component (a2) is 100% by mass.

[0039] The component (a2) excludes hydrogenated products of block copolymers composed of a polymer block mainly composed of an aromatic vinyl compound and a random copolymer block of a conjugated diene compound and an aromatic vinyl compound.

[0040] The 14th invention is the method according to the 13th invention, wherein the component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms.

[0041] The fifteenth invention is a method for producing an adhesive coating, comprising: a step (1) of producing a thermoplastic resin composition by the method described in the thirteenth invention or the fourteenth invention, and a step (2) of dissolving the thermoplastic resin composition obtained in the step (1) in a solvent.

[0042] The sixteenth invention is an extruded packaged product comprising the laminate according to any one of the seventh to twelfth inventions.

[0043] The 17th invention is a method for producing an extruded packaged product, comprising: a step (1) of producing a thermoplastic resin composition using the method described in the 13th invention or the 14th invention; a step (3) of producing a laminate using the thermoplastic resin composition obtained in the above step (1); and a step (4) of producing an extruded packaged product using the laminate obtained in the above step.

[0044] The thermoplastic resin composition of the present invention can bond cyclic polyolefin polymer and ethylene-vinyl alcohol copolymer with sufficient strength. In addition, it is excellent in impact resistance and will not damage the characteristics of cyclic polyolefin polymer and ethylene-vinyl alcohol copolymer. Therefore, by using the thermoplastic resin composition of the present invention as an adhesive component by coextrusion or as an adhesive coating coating method to make it between the two, a laminate of the two can be obtained with high productivity. Furthermore, the productivity of the thermoplastic resin composition of the present invention as a composition is also excellent.

[0045] The thermoplastic resin composition of the present invention can bond the cyclic polyolefin polymer and the metal or metal compound such as aluminum foil with sufficient strength. In addition, the properties of the cyclic polyolefin polymer and the metal or metal compound such as aluminum foil are not impaired. Therefore, by using the thermoplastic resin composition of the present invention as an adhesive component and placing it between the two, a laminate of the two can be obtained with high productivity. DETAILED DESCRIPTION

[0046] In this specification, the term "film" is used as a term that also includes sheets. The term "resin" is used as a term that also includes a resin mixture containing two or more resins, or a resin composition containing components other than resins. "Laminating a certain layer and other layers" includes both directly laminating these layers and laminating them with one or more other layers such as anchor coatings interposed between these layers. The term "above" in the numerical range is used with a certain value or a value exceeding a certain value. For example, more than 20% means 20% or more than 20%. The term "below" in the numerical range is used with a certain value or a value below a certain value. For example, less than 20% means 20% or less than 20%. Furthermore, the symbol "~" in the numerical range is used with a certain value, a value exceeding a certain value and less than another certain value, or another certain value. Here, another certain value is set to a value greater than a certain value. For example, 10 to 90% means 10%, more than 10% and less than 90%, or 90%.

[0047] The thermoplastic resin composition of the present invention contains (A) 100 parts by mass of a thermoplastic resin, (B) 0.05 to 5 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic acid derivatives, and (C) 0.01 to 3 parts by mass of an organic peroxide.

[0048] (A) Thermoplastic resin:

[0049] The above-mentioned component (A) comprises: (a1) cyclic polyolefin polymer 10~90 mass % and (a2) one or more 90~10 mass % selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds and hydrogenated products thereof. Preferably, the above-mentioned component (a1) 40~80 mass % and the above-mentioned component (a2) 60~20 mass % are included. Here, the total of the above-mentioned component (a1) and the above-mentioned component (a2) is 100 mass %. In addition, in this specification, the hydrogenated product of the block copolymer consisting of the polymer block with aromatic vinyl compounds as the main body and the random copolymer block of conjugated diene compounds and aromatic vinyl compounds is excluded from the above-mentioned component (a2).

[0050] When the content of the component (a1) is 10% by mass or more, preferably 40% by mass or more (the content of the component (a2) is 90% by mass or less, preferably 60% by mass or less), the adhesiveness becomes good. When the content of the component (a1) is 90% by mass or less, preferably 80% by mass or less (the content of the component (a2) is 10% by mass or more, preferably 20% by mass or more), the impact resistance becomes good.

[0051] (a1) Cyclic polyolefin polymers:

[0052] The above-mentioned component (a1) is a polymer mainly containing structural units (usually 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more) derived from cyclic olefins (polymerizable compounds having a cyclic structure formed by carbon atoms and having ethylenic carbon-carbon double bonds in the ring).

[0053] Examples of the cyclic olefins include cyclobutene, cyclopentene, cyclopentadiene, norbornene (bicyclo[2.2.1]hept-2-ene), dicyclopentadiene (tricyclo[4.3.0.12,5]deca-3,7-diene), tetracyclododecene (tetracyclo[4.4.0.12,5.17,10]dec-3-ene), and derivatives thereof.

[0054] The cyclic polyolefin polymer can be produced by a known polymerization method using one or more of the cyclic olefins described above. In this case, one or more other monomers copolymerizable with the cyclic olefin can be used.

[0055] Examples of the other monomers include α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 2-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-hexadecene, and 1-eicosene; and non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene.

[0056] As the component (a1), from the viewpoint of adhesiveness, a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms (e.g., ethylene, propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene) is preferred. A copolymer of one or more selected from the group consisting of norbornene and its derivatives and an α-olefin having 2 to 8 carbon atoms is more preferred.

[0057] The glass transition temperature of the component (a1) is preferably 70 to 160° C., more preferably 75 to 140° C. When the glass transition temperature is 70° C. or higher, heat resistance becomes good, and when the glass transition temperature is 160° C. or lower, productivity as a composition becomes good.

[0058] In this specification, the glass transition temperature is the midpoint glass transition temperature calculated from the curve of the final heating process measured according to JIS K7121-1987 using a Diamond DSC differential scanning calorimeter manufactured by PerkinElmer Japan Co., Ltd., and is a procedure of holding at 350° C. for 5 minutes, cooling to 30° C. at 10° C. / min, holding at 30° C. for 3 minutes, and heating to 350° C. at 10° C. / min.

[0059] The melt flow rate (hereinafter referred to as "MFR") of the component (a1) measured at 260°C and 21.18 N according to JIS K7210-1999 is preferably 0.1 to 50 g / 10 min, more preferably 1 to 20 g / 10 min. When the MFR is within the above range, moldability is improved.

[0060] Examples of commercially available products of the component (a1) include "TOPAS 8007", "TOPAS 6013", and "TOPAS 6015" from Polyplastics Co., Ltd., "APEL APL 6013T" and "APEL APL 6015T" from Mitsui Chemicals, Inc., and "ZEONOR 1020R" and "ZEONOR 1060R" from Zeon Corporation.

[0061] As the component (a1), one or more of these substances can be used.

[0062] (a2) Copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof:

[0063] The above-mentioned component (a2) is one or more selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof. However, the hydrogenated product of the block copolymer consisting of a polymer block with an aromatic vinyl compound as the main body and a random copolymer block of a conjugated diene compound and an aromatic vinyl compound is excluded from the above-mentioned component (a2). Here, "a polymer block with an aromatic vinyl compound as the main body" means that the content of the structural unit derived from the aromatic vinyl compound in the polymer block is usually 90% by mass or more. In addition, "a random copolymer block of a conjugated diene compound and an aromatic vinyl compound" usually means a significant amount of a conjugated diene compound and a significant amount of an aromatic vinyl compound. The random copolymer block is typically composed of 10 to 97% by mass of a structural unit derived from a conjugated diene compound and 90 to 3% by mass of a structural unit derived from an aromatic vinyl compound. Here, the sum of the content of the structural unit derived from the conjugated diene compound and the content of the structural unit derived from the aromatic vinyl compound is 100% by mass.

[0064] Examples of the copolymer of the aromatic vinyl compound and the conjugated diene compound or its hydrogenated product include: a block copolymer of the aromatic vinyl compound and the conjugated diene compound, a hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound, a random copolymer of the aromatic vinyl compound and the conjugated diene compound, and a hydrogenated product of the random copolymer of the aromatic vinyl compound and the conjugated diene compound.

[0065] The aromatic vinyl compound is a polymerizable monomer having a polymerizable carbon-carbon double bond and an aromatic ring. Examples of the aromatic vinyl compound include styrene, tert-butylstyrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, vinyltoluene, and p-tert-butylstyrene. Among these compounds, styrene is preferred. As the aromatic vinyl compound, one of these compounds or a combination of two or more thereof may be used.

[0066] The above-mentioned conjugated diene is a polymerizable monomer having a structure in which two carbon-carbon double bonds are bonded by one carbon-carbon single bond. As the conjugated diene, for example, 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, and chloroprene (2-chloro-1,3-butadiene) can be cited. Among these compounds, 1,3-butadiene and isoprene are preferred. As the above-mentioned conjugated diene, one of these compounds can be used or two or more of them can be used in combination.

[0067] The block copolymer of the aromatic vinyl compound and the conjugated diene compound is a block copolymer composed of at least one, preferably two or more, polymer block A with the aromatic vinyl compound as the main body and at least one polymer block B with the conjugated diene compound as the main body. For example, block copolymers of aromatic vinyl compounds and conjugated diene compounds having structures such as AB, ABA, BABA, ABABA, etc. can be cited. The block copolymer can usually contain 5 to 60% by mass, preferably 20 to 50% by mass, of structural units derived from aromatic vinyl compounds.

[0068] The polymer block A is a polymer block consisting only of an aromatic vinyl compound; or a copolymer block of an aromatic vinyl compound and a conjugated diene compound. When the polymer block A is a copolymer block, the content of the structural unit derived from the aromatic vinyl compound in the polymer block A can usually be 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more. The distribution of the structural unit derived from the conjugated diene compound in the polymer block A is not particularly limited and is arbitrary. When the polymer block A is 2 or more, these may be the same structure or different structures from each other.

[0069] The polymer block B is a polymer block consisting only of a conjugated diene compound; or a copolymer block of an aromatic vinyl compound and a conjugated diene compound. The content of the structural unit derived from the conjugated diene compound in the polymer block B when the polymer block B is a copolymer block is usually 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more. The distribution of the structural unit derived from the aromatic vinyl compound in the polymer block B is not particularly limited and is arbitrary. The bonding mode of the conjugated diene compound and the conjugated diene compound (hereinafter, sometimes referred to as microstructure) is not particularly limited and is arbitrary. When the polymer block B is 2 or more, these may be the same structure or different structures from each other.

[0070] The number average molecular weight of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is preferably 5,000 to 1,500,000, more preferably 10,000 to 550,000, and further preferably 100,000 to 400,000. The molecular weight distribution (mass average molecular weight / number average molecular weight) is preferably 10 or less. The molecular chain structure of the block copolymer of the aromatic vinyl compound and the conjugated diene compound may be any one of linear, branched, radial, and any combination thereof. It should be noted that the mass average molecular weight (Mw) and the number average molecular weight (Mn) refer to polystyrene conversion values ​​using gel permeation chromatography (GPC).

[0071] Examples of the block copolymer of the aromatic vinyl compound and the conjugated diene compound include styrene-butadiene-styrene block copolymer (SBS) and styrene-isoprene-styrene block copolymer (SIS).

[0072] The block copolymer of the aromatic vinyl compound and the conjugated diene compound is not particularly limited, and may be a block copolymer obtained by copolymerizing any aromatic vinyl compound and any conjugated diene by a known method such as the method described in Japanese Patent Publication No. 40-023798.

[0073] The hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is obtained by adding hydrogen to the carbon-carbon double bonds in the block copolymer of the aromatic vinyl compound and the conjugated diene compound to form carbon-carbon single bonds. The hydrogenation can be carried out by a known method, for example, by hydrogenation treatment using a hydrogenation catalyst in an inert solvent.

[0074] The hydrogenation rate of the hydrogenated product of the block copolymer of the above-mentioned aromatic vinyl compound and conjugated diene compound (the ratio of the number of carbon-carbon double bonds in the block copolymer of the aromatic vinyl compound and the conjugated diene compound before hydrogenation to the number of carbon-carbon single bonds converted by hydrogenation) is not particularly limited, and from the viewpoint of permeation resistance, it can usually be 50% or more, preferably 70% or more, and more preferably 90% or more.

[0075] When the conjugated diene polymer block of the hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is a butadiene polymer block, the 1,2-bond content is preferably 20 to 50% by mass, more preferably 25 to 45% by mass, in terms of its microstructure from the viewpoint of impact resistance. In addition, from the viewpoint of heat aging resistance and weather resistance, the 1,2-bond may be selectively hydrogenated.

[0076] When the conjugated diene polymer block of the hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is a copolymer block of isoprene and butadiene, the 1,2-bond content is preferably less than 50%, more preferably less than 25%, and further preferably less than 15% in terms of its microstructure from the viewpoint of heat aging resistance and weather resistance.

[0077] When the conjugated diene polymer block of the hydrogenated block copolymer of an aromatic vinyl compound and a conjugated diene compound is an isoprene polymer block, the microstructure preferably has 70 to 100% by mass of 1,4 bonds from the viewpoint of impact resistance, and the hydrogenation rate is preferably 90% or more from the viewpoint of permeation resistance.

[0078] From the viewpoint of mechanical physical properties, the content of the structural unit derived from the aromatic vinyl compound in the hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is preferably 5 to 70% by mass, more preferably 20 to 50% by mass. From the viewpoint of permeation resistance, the number average molecular weight of the hydrogenated product of the block copolymer of the aromatic vinyl compound and the conjugated diene compound is preferably 30,000 or more, more preferably 100,000 or more. From the viewpoint of compatibility, it is preferably 350,000 or less, more preferably 250,000 or less.

[0079] Examples of hydrogenated products of block copolymers of the above-mentioned aromatic vinyl compounds and conjugated diene compounds include styrene·ethylene·butylene copolymer (SEB), styrene·ethylene·propylene copolymer (SEP), styrene·ethylene·butylene·styrene copolymer (SEBS), styrene·ethylene·propylene·styrene copolymer (SEPS), styrene·ethylene·ethylene·propylene·styrene copolymer (SEEPS), styrene·butadiene·butylene·styrene copolymer (partially hydrogenated product of styrene·butadiene·styrene copolymer: SBBS), partially hydrogenated products of styrene·isoprene·styrene copolymer, and partially hydrogenated products of styrene·isoprene·butadiene·styrene copolymer.

[0080] For the random copolymer of the above-mentioned aromatic vinyl compound and conjugated diene compound, from the viewpoint of mechanical strength, it can be a substance containing a structural unit derived from an aromatic vinyl compound preferably more than 3 mass %, more preferably more than 5 mass % (a structural unit derived from a conjugated diene compound preferably less than 97 mass %, more preferably less than 95 mass %). On the other hand, from the viewpoint of impact resistance, it can be a substance containing a structural unit derived from an aromatic vinyl compound preferably less than 60 mass %, more preferably less than 50 mass % (a structural unit derived from a conjugated diene compound preferably more than 40 mass %, more preferably more than 50 mass %). Here, the sum of the structural unit derived from an aromatic vinyl compound and the structural unit derived from a conjugated diene compound is 100 mass %.

[0081] The random copolymer of the aromatic vinyl compound and the conjugated diene compound may preferably have a number average molecular weight of 150,000 to 500,000, more preferably 170,000 to 400,000, and still more preferably 200,000 to 350,000. The molecular weight distribution (mass average molecular weight / number average molecular weight) is preferably 10 or less.

[0082] Examples of the random copolymer of the aromatic vinyl compound and the conjugated diene compound include a random copolymer of styrene and butadiene (SBR).

[0083] The hydrogenated product of the random copolymer of the aromatic vinyl compound and the conjugated diene compound is produced by hydrogenating the random copolymer of the aromatic vinyl compound and the conjugated diene compound. The hydrogenation rate (the ratio of the number of carbon-carbon double bonds in the random copolymer of the aromatic vinyl compound and the conjugated diene compound before hydrogenation to the number of carbon-carbon single bonds converted by hydrogenation) is not particularly limited and can usually be 90% or more, preferably 99% or more.

[0084] Examples of the hydrogenated product of the random copolymer of an aromatic vinyl compound and a conjugated diene compound include a hydrogenated product of a random copolymer of styrene and butadiene (HSBR).

[0085] As component (a2) contained in the thermoplastic resin composition of the present invention, preferred are hydrogenated products of block copolymers of an aromatic vinyl compound and a conjugated diene compound and hydrogenated products of random copolymers of an aromatic vinyl compound and a conjugated diene compound, and more preferred are hydrogenated products of block copolymers of an aromatic vinyl compound and a conjugated diene compound.

[0086] As the component (a2), these compounds may be used alone or in mixture of two or more.

[0087] It should be noted that the copolymer of the aromatic vinyl compound and the conjugated diene compound and / or its hydrogenated product may contain structural units derived from the aromatic vinyl compound and a polymerizable compound other than the conjugated diene compound, within the limits not contradicting the purpose of the present invention.

[0088] Examples of the polymerizable compound include α-olefins such as ethylene, propylene, 1-butene, 1-hexene, and 1-octene; non-conjugated dienes such as isobutylene; (meth)acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; and maleic anhydride.

[0089] (B) Unsaturated carboxylic acids and their derivatives:

[0090] The component (B) is one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids. The component (B) is graft polymerized with the component (A) to impart adhesion to the thermoplastic resin composition of the present invention to resins or metals having polar groups such as ethylene-vinyl alcohol copolymer (EVOH), nylon, and polyester.

[0091] Examples of the unsaturated carboxylic acid include maleic acid, itaconic acid, fumaric acid, acrylic acid, and methacrylic acid. Examples of the derivatives of the unsaturated carboxylic acid include maleic acid monoesters, maleic acid diesters, maleic anhydride, itaconic acid monoesters, itaconic acid diesters, itaconic anhydride, fumaric acid monoesters, fumaric acid diesters, fumaric anhydride, alkyl acrylates such as methyl acrylate, and alkyl methacrylates such as methyl methacrylate. As the component (B), one or a mixture of two or more of these compounds may be used.

[0092] As the component (B), maleic anhydride is preferred from the viewpoint of reactivity with the component (A) and adhesion of the composition.

[0093] The amount of the component (B) is 0.05 to 5 parts by mass relative to 100 parts by mass of the component (A). From the viewpoint of improving the adhesiveness of the thermoplastic resin of the present invention, the amount is 0.05 parts by mass or more, preferably 0.1 parts by mass or more. In addition, from the viewpoint of preventing the component (B) from remaining in the composition without reacting during modification (graft polymerization), causing the color tone of the article composed of the composition to change (yellowing) or gelling, etc., the amount is 5 parts by mass or less, preferably 3 parts by mass or less.

[0094] (C) Organic peroxide

[0095] The component (C) of the present invention is an organic peroxide, and plays a role in catalyzing the graft polymerization reaction of the above-mentioned components (A) and (B).

[0096] Examples of the organic peroxide include diisopropylbenzene peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butylperoxybenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylisopropylbenzene peroxide. As the component (C), one or a mixture of two or more of these compounds may be used.

[0097] As the component (C), from the viewpoint of the productivity and adhesiveness of the composition, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane and 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3 are preferred.

[0098] The amount of the component (C) is 0.001 to 3 parts by mass relative to 100 parts by mass of the component (A). From the viewpoint of improving the adhesiveness of the thermoplastic resin composition of the present invention and preventing the formation of gel during film formation, the amount is 0.001 parts by mass or more, preferably 0.03 parts by mass or more. From the viewpoint of suppressing the change in color tone (yellowing) or the decrease in melt viscosity during modification, the amount is 3 parts by mass or less, preferably 2 parts by mass or less.

[0099] Examples of commercially available products of the component (C) include "PERHEXA25B (trade name)" and "PERHEXANE25B (trade name)" from NOF Corporation.

[0100] The thermoplastic resin composition of the present invention may further contain components other than the above-mentioned components (A) to (C), for example, thermoplastic resins other than the above-mentioned component (A); pigments, inorganic fillers, organic fillers, resin fillers; additives such as lubricants, antioxidants, weather stabilizers, heat stabilizers, release agents, antistatic agents, and surfactants, etc., as desired, within the limits not contrary to the purpose of the present invention.

[0101] Production of thermoplastic resin composition:

[0102] The thermoplastic resin composition of the present invention can be obtained by melt-kneading the above-mentioned components (A) to (C) and any desired optional components using any melt-kneading machine.

[0103] The thermoplastic resin composition can be obtained by melt-kneading the components (A) to (C) and any desired component using any melt kneader, preferably at a temperature higher than the 1-minute half-life temperature of the component (C) for 1 minute or more, more preferably at a temperature higher than the 1-minute half-life temperature of the component (C) for 2 minutes or more. It should be noted that the 1-minute half-life temperature refers to a temperature at which the half-life becomes 1 minute, meaning that when the -OO- bond in the component (C) is decomposed at this temperature, the time required for the current concentration of the bond to become half of the initial concentration is 1 minute.

[0104] The melt kneading machine is not particularly limited, and examples thereof include a single-screw extruder, a twin-screw extruder, a Banbury mixer, various kneaders, and a combination of two or more of these.

[0105] From the viewpoint of improving the manufacturability in the subsequent melt kneading step, the melt mass flow rate of the thermoplastic resin composition measured in accordance with JIS K7210:1999 at 230° C. and 21.18 N is preferably 0.5 g / 10 min or more. From the viewpoint of the moldability when a laminate is molded using the thermoplastic resin composition or the adhesiveness of the composition, it is preferably 15 g / 10 min or less.

[0106] The above-mentioned thermoplastic resin composition introduces polar groups such as carboxyl groups into the cyclic polyolefin-based non-polar materials, and exhibits good adhesion to various materials. Examples of non-polar materials that exhibit good adhesion include polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, and cyclic polyolefins. Examples of polar materials include resins having polar groups such as ethylene-vinyl alcohol copolymer (EVOH), nylon, polyurethane, and polyester; and metals such as iron, aluminum, copper, silver, gold, and tin; metal compounds (inorganic metal compounds) such as oxides, nitrides, fluorides, and sulfides of one or more metals such as aluminum, tin, zinc, indium, germanium, antimony, and cerium; etc. Surprisingly, it was found that good adhesion was exhibited, in particular, to polyolefins and ethylene-vinyl alcohol copolymers having a large number of hydroxyl groups. Therefore, the thermoplastic resin composition of the present invention is suitable for use as an adhesive material.

[0107] Adhesive coating

[0108] The adhesive coating material of the present invention can be obtained by dissolving the thermoplastic resin composition of the present invention in a solvent by any method.

[0109] As the above-mentioned solvent, there is no particular limitation as long as it is a solvent that can dissolve the thermoplastic resin composition of the present invention, and any solvent can be used. As the above-mentioned solvent, for example, toluene, xylene, methyl isobutyl ketone, cyclohexane, methylcyclohexane, tetrahydrofuran, and chloroform can be mentioned. Among these compounds, toluene and cyclohexane are preferred from the viewpoint of solubility and storage stability. As the above-mentioned solvent, one or more of these substances can be used.

[0110] The amount of the solvent to be added also depends on the thickness of the coating film formed using the adhesive coating of the present invention, but in the case of a commonly used coating device, it can usually be 100 to 2000 parts by mass, preferably 300 to 1800 parts by mass, and more preferably 500 to 1500 parts by mass, relative to 100 parts by mass of the component (A).

[0111] The adhesive coating of the present invention may further contain the above-mentioned components (A) to (C) and components other than the above-mentioned solvent, for example, thermoplastic resins other than the above-mentioned component (A); pigments, inorganic fillers, organic fillers, resin fillers; additives such as lubricants, antioxidants, weather stabilizers, heat stabilizers, release agents, antistatic agents, and surfactants, etc., as needed, within the limits not violating the purpose of the present invention.

[0112] Laminated body

[0113] Preferred articles produced using the thermoplastic resin composition of the present invention include a laminate having at least one layer composed of the thermoplastic resin composition of the present invention.

[0114] The thickness of the layer composed of the thermoplastic resin composition of the present invention may be generally 1 μm or more, preferably 2 μm or more from the viewpoint of adhesiveness, and generally 100 μm or less, preferably 30 μm or less from the viewpoint of economic efficiency.

[0115] Furthermore, from the viewpoints of the manufacturability, mechanical strength, and web controllability of the laminate, the total thickness of the laminate may be generally 10 to 1000 μm, preferably 20 to 500 μm.

[0116] Preferred embodiments of the above-mentioned laminate include, for example: a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a resin having a polar group are laminated in this order; and a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, a layer composed of a resin having a polar group, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a cyclic polyolefin polymer are laminated in this order.

[0117] As more preferred embodiments of the above-mentioned laminate, for example, there can be mentioned a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a resin having a polar group are directly laminated in this order; and a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, a layer composed of a resin having a polar group, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a cyclic polyolefin polymer are directly laminated in this order.

[0118] The layer composed of the resin having a polar group in the laminate is preferably a layer composed of an ethylene-vinyl alcohol copolymer.

[0119] The method for manufacturing the above-mentioned laminate is not particularly limited, and any device and method can be used for manufacturing. As the above-mentioned method, for example, the following can be cited: a method of melting the constituent materials of each layer with each extruder, and performing T-die co-extrusion using a multi-channel manifold method, a stack plate method, or a feed block method; an extrusion lamination method in which at least one resin film is obtained by any method, and other resin layers are melt-extruded on the film; a method in which the resin films of each layer are obtained by any method and then integrated by heat lamination; and a method in which a film of a cyclic polyolefin polymer and a film of a resin having a polar group are obtained by any method, and then dry-lamination is performed using the adhesive coating of the present invention, etc.

[0120] The laminate of the above-described embodiment of the laminate of the present invention is a laminate having high strength, high gas barrier properties, and chemical resistance, and can be preferably used as a packaging film or storage container for food or medical devices, for example.

[0121] As other preferred embodiments of the laminate of the present invention, for example, there can be mentioned a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a metal or a metal compound are laminated in this order; and a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, a layer composed of a metal or a metal compound, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a cyclic polyolefin polymer are laminated in this order.

[0122] As more preferred embodiments of the above-mentioned laminate, for example, there can be mentioned a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a metal or a metal compound are directly laminated in this order; and a laminate in which a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition of the present invention, a layer composed of a metal or a metal compound, a layer composed of the thermoplastic resin composition of the present invention, and a layer composed of a cyclic polyolefin polymer are directly laminated in this order.

[0123] The layer composed of a metal or a metal compound in the laminate is preferably a layer composed of an aluminum foil.

[0124] The method for producing the laminate is not particularly limited, and the laminate can be produced using any device and any method. Examples of the method include: an extrusion lamination method in which a laminate having a layer composed of a cyclic polyolefin polymer and a layer composed of the thermoplastic resin composition of the present invention is melt-extruded on a foil composed of a metal or a metal compound in such a manner that the layer composed of the thermoplastic resin composition of the present invention is on the foil side; a method in which a laminate having a layer composed of a cyclic polyolefin polymer and a layer composed of the thermoplastic resin composition of the present invention is obtained by any method, and then heat-laminated in such a manner that the foil and the layer composed of the thermoplastic resin composition of the present invention are on the foil side; and a method in which a film of a cyclic polyolefin polymer is obtained by any method, and then dry-laminated using the foil and the adhesive coating of the present invention; etc.

[0125] Examples of the above method include: an extrusion lamination method in which a laminate having a layer composed of a cyclic polyolefin polymer and a layer composed of the thermoplastic resin composition of the present invention is melt-extruded on a layer composed of a metal or a metal compound in a laminate having a layer composed of a metal or a metal compound on at least one surface thereof so that the layer composed of the thermoplastic resin composition of the present invention is on the side of the layer composed of the metal or the metal compound; a method in which a laminate having a layer composed of a cyclic polyolefin polymer and a layer composed of the thermoplastic resin composition of the present invention is obtained by an arbitrary method and then heat-laminated so that the laminate having a layer composed of a metal or a metal compound on at least one surface thereof and the layer composed of the thermoplastic resin composition of the present invention are on the side of the layer composed of the metal or the metal compound; and the like.

[0126] Examples of laminates having a layer composed of a metal or a metal compound on at least one surface thereof include: a laminate formed by laminating an arbitrary film-like substrate and a foil composed of a metal or a metal compound by dry lamination, hot lamination, or the like; a laminate formed by vapor-depositing a metal or a metal compound on an arbitrary film-like substrate by an arbitrary method; a laminate formed by melt-extruding an arbitrary thermoplastic resin on a foil composed of a metal or a metal compound; and a laminate in which a coating is formed on a foil composed of a metal or a metal compound using an arbitrary coating agent; etc.

[0127] The laminate of the above-described embodiment of the laminate of the present invention has extremely high gas barrier properties and can be preferably used as a packaging film or storage container for contents that are not resistant to oxygen or moisture, such as food, medical instruments, and pharmaceuticals.

[0128] Examples of products using the laminate of the present invention as packaging films or storage containers include extruded packaging products.

[0129] Example

[0130] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples.

[0131] Determination method

[0132] (1) Adhesion:

[0133] (1-1) Cyclic polyolefin copolymers:

[0134] Using a 40 mm single-screw extruder, the adhesive composition obtained in the following steps is extruded from a two-color molding die head using a 25 mm single-screw extruder at a mold temperature of 240°C. The cross-sectional shape when cut in a direction perpendicular to the machine direction is generally rectangular, and a two-color molded product having a rectangular layer of a cyclic polyolefin copolymer of the same shape and a thickness of 0.1 mm is formed on a layer of the adhesive composition of the same shape and a thickness of 1 mm. A sample with a width of 15 mm was cut near the center in the width direction of the two-color molded product obtained in the above steps, and the 180-degree peeling adhesion of the cyclic polyolefin copolymer layer relative to the adhesive composition layer was measured at a test speed of 300 mm / min, with the adhesive composition layer as the test plate and the cyclic polyolefin copolymer layer as the adhesive tape, with reference to 10.4 of JIS Z0237:2009. It should be noted that in the case where the adhesiveness is very high and the starting point of peeling cannot be made, it is recorded as ">>" in the table.

[0135] (1-2) Ethylene-vinyl alcohol copolymer:

[0136] The adhesive composition obtained in the following step was extruded from an ethylene-vinyl alcohol copolymer ("EVAL L-171B (trade name)" of Kuraray Co., Ltd.) through a two-color molding die head at a die temperature of 200°C using a 40 mm single screw extruder, and a two-color molded article having a rectangular cross-sectional shape when cut in a direction perpendicular to the machine direction and a rectangular adhesive composition layer having a thickness of 1 mm and a rectangular ethylene-vinyl alcohol copolymer layer having the same shape and a thickness of 0.1 mm was formed. A sample having a width of 15 mm was cut near the center in the width direction of the two-color molded article obtained in the above step, and the 180-degree peel adhesion of the ethylene-vinyl alcohol copolymer layer to the adhesive composition layer was measured at a test speed of 300 mm / min, with the adhesive composition layer as a test plate and the ethylene-vinyl alcohol copolymer layer as an adhesive tape.

[0137] (1-3) For metal foil:

[0138] The adhesive composition obtained in the following step was extruded into a thickness of 1 mm on a 25 μm aluminum foil (untreated aluminum foil of UACJ Co., Ltd.) using a 40 mm single screw extruder at a die temperature of 200° C. and laminated. A sample with a width of 15 mm was cut from the center of the laminate obtained in the above step in the width direction, and the 180-degree peeling adhesion of the metal foil layer to the adhesive composition layer was measured at a test speed of 300 mm / min, with the adhesive composition layer as a test plate and the metal foil layer as an adhesive tape, with reference to 10.4 of JIS Z0237:2009.

[0139] (2) Impact resistance (Izod impact strength):

[0140] Using an injection molding machine with a clamping pressure of 125 tons, a 1 / 4 inch thick injection sheet molded at a drum temperature of 260 to 280°C and a metal mold temperature of 30°C was used as a test piece, and the Izod impact strength (with notch) was measured according to ASTM D256. It should be noted that the case where the test piece has no cracks is recorded as NB.

[0141] (3) Particle production rate:

[0142] The pellets obtained by the strand cutting method of the adhesive composition were visually observed and evaluated according to the following criteria.

[0143] ○: The particle shape is good.

[0144] ×: At least one of the following defects occurred.

[0145] The particles are in clumps.

[0146] The particles are irregular in shape.

[0147] Penetration of ingredients can be seen in the particles.

[0148] Raw materials used

[0149] Ingredients (a1):

[0150] (a1-1) Cyclic olefin copolymer "TOPAS 8007F-04 (trade name)" manufactured by Polyplastics Co., Ltd., glass transition temperature: 79°C, MFR (260°C, 2.16 kg): 32 g / 10 min.

[0151] (a1-2) Cyclic olefin copolymer "TOPAS 6013F-04 (trade name)" manufactured by Polyplastics Co., Ltd., glass transition temperature: 139°C, MFR (260°C, 2.16 kg): 14 g / 10 min.

[0152] (a1-3) Cyclic olefin copolymer "APEL 6013T (trade name)" manufactured by Mitsui Chemicals, Inc., glass transition temperature: 125°C, MFR (260°C, 2.16 kg): 14 g / 10 min.

[0153] (a1-4) Cycloolefin polymer "ZEONOR 1020R (trade name)" manufactured by Zeon Corporation of Japan, glass transition temperature: 102°C, MFR (280°C, 21.18N): 20 g / 10 min.

[0154] Ingredient (a2):

[0155] (a2-1) TUFTECH 1052 (trade name) a block copolymer of styrene, ethylene, butadiene and styrene produced by Asahi Kasei Corporation, with a hydrogenation rate of 90 mol% or more and a content of structural units derived from styrene of 20% by mass.

[0156] (a2-2) "SEPTON 2002 (trade name)" a block copolymer of styrene, ethylene, propylene and styrene manufactured by Kuraray Co., Ltd., with a hydrogenation rate of 90 mol% or more and a content of structural units derived from styrene of 30% by mass.

[0157] (a2-3) A hydrogenated product of a random copolymer composed of 1,3-butadiene and styrene, "DYNARON 1320P (trade name)" manufactured by JSR Corporation, with a hydrogenation rate of 99 mol% and a content of structural units derived from styrene of 10% by mass.

[0158] Ingredient (B):

[0159] (B-1) Maleic anhydride produced by Nippon Catalyst Co., Ltd.

[0160] Ingredients (C):

[0161] (C-1) 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane "PERHEXA25B (trade name)" manufactured by NOF Corporation, 1-minute half-life temperature: 180°C.

[0162] Examples 1 to 19

[0163] A co-rotating twin-screw extruder was used to batch feed a mixture of any of the formulations (parts by mass) shown in Tables 1 to 3, and melt-kneaded the mixture at an extruder outlet resin temperature of 190° C., thereby obtaining an adhesive composition. The obtained adhesive composition was subjected to the above-mentioned evaluations (1) to (3). The results are shown in any of Tables 1 to 3.

[0164] [Table 1]

[0165]

[0166] [Table 2]

[0167]

[0168] [Table 3]

[0169]

[0170] The thermoplastic resin composition (adhesive composition) of the present invention is excellent in adhesiveness and impact resistance, has excellent productivity as a composition, and has a good shape of the obtained pellets.

Claims

1. A thermoplastic resin composition comprising: (A) 100 parts by mass of a thermoplastic resin; (B) 0.2 to 4 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids; and (C) 0.02 to 3 parts by mass of an organic peroxide, The (A) thermoplastic resin comprises: (a1) 40 to 80% by mass of a cyclic polyolefin polymer; and (a2) 60 to 20% by mass of one or more selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof, Here, the total amount of the component (a1) and the component (a2) is 100% by mass. The glass transition temperature of the cyclic polyolefin polymer (a1) is 70 to 160° C., The component (a2) excludes hydrogenated products of block copolymers composed of polymer blocks mainly composed of aromatic vinyl compounds and random copolymer blocks of conjugated diene compounds and aromatic vinyl compounds, The unsaturated carboxylic acid derivative of the component (B) is selected from the group consisting of maleic acid monoesters, maleic acid diesters, maleic acid anhydride, itaconic acid monoesters, itaconic acid diesters, itaconic acid anhydride, fumaric acid monoesters, fumaric acid diesters, fumaric acid anhydride, alkyl acrylates, and alkyl methacrylates.

2. The thermoplastic resin composition according to claim 1, wherein The component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms.

3. The thermoplastic resin composition according to claim 1, wherein The component (a2) is a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

4. A thermoplastic resin composition comprising: (A) 100 parts by mass of a thermoplastic resin; (B) 0.2 to 4 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids; and (C) 0.02 to 3 parts by mass of an organic peroxide, The (A) thermoplastic resin comprises: (a1) 40 to 80% by mass of a cyclic polyolefin polymer; and (a2-2) 60 to 20% by mass of a hydrogenated product of a random copolymer of an aromatic vinyl compound and a conjugated diene compound, Here, the total amount of the component (a1) and the component (a2-2) is 100% by mass. The unsaturated carboxylic acid derivative of the component (B) is selected from the group consisting of maleic acid monoesters, maleic acid diesters, maleic acid anhydride, itaconic acid monoesters, itaconic acid diesters, itaconic acid anhydride, fumaric acid monoesters, fumaric acid diesters, fumaric acid anhydride, alkyl acrylates, and alkyl methacrylates.

5. The thermoplastic resin composition according to claim 4, wherein The glass transition temperature of the (a1) cyclic polyolefin polymer is 70 to 160°C. 6 . An adhesive coating material comprising the thermoplastic resin composition according to claim 1 .

7. The coating according to claim 6, wherein The component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms, The amount of the structural unit derived from the cyclic olefin is 50% by mass or more. 8 . A laminate comprising at least one layer comprising the thermoplastic resin composition according to claim 1 . 9 . A laminated body comprising a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to claim 1 , and a layer composed of a resin having a polar group laminated in this order.

10. A laminated body comprising a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to any one of claims 1 to 5, a layer composed of a resin having a polar group, a layer composed of the thermoplastic resin composition according to any one of claims 1 to 4, and a layer composed of a cyclic polyolefin polymer laminated in this order.

11. The laminate according to claim 9, wherein The resin having polar groups is ethylene-vinyl alcohol copolymer. 12 . A laminated body comprising a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to claim 1 , and a layer composed of a metal or a metal compound laminated in this order.

13. A laminated body, comprising a layer composed of a cyclic polyolefin polymer, a layer composed of the thermoplastic resin composition according to any one of claims 1 to 5, a layer composed of a metal or a metal compound, a layer composed of the thermoplastic resin composition according to any one of claims 1 to 5, and a layer composed of a cyclic polyolefin polymer laminated in this order.

14. The laminate according to claim 12, wherein The layer composed of metal or metal compound is a layer composed of aluminum foil. 15 . A packaging film or a storage container comprising the thermoplastic resin composition according to claim 1 .

16. An extrusion-packaged product comprising the laminate according to any one of claims 8 to 14.

17. A method for producing a thermoplastic resin composition, comprising the step of melt-kneading a thermoplastic resin composition, wherein the composition comprises: (A) 100 parts by mass of a thermoplastic resin, (B) 0.2 to 4 parts by mass of one or more selected from the group consisting of unsaturated carboxylic acids and derivatives of unsaturated carboxylic acids, and (C) 0.02 to 3 parts by mass of an organic peroxide, The (A) thermoplastic resin comprises: (a1) 40 to 80% by mass of a cyclic polyolefin polymer, (a2) 60 to 20% by mass of one or more selected from the group consisting of copolymers of aromatic vinyl compounds and conjugated diene compounds, and hydrogenated products thereof, Here, the total amount of the component (a1) and the component (a2) is 100% by mass. The glass transition temperature of the cyclic polyolefin polymer (a1) is 70 to 160° C., The component (a2) excludes hydrogenated products of block copolymers composed of polymer blocks mainly composed of aromatic vinyl compounds and random copolymer blocks of conjugated diene compounds and aromatic vinyl compounds, The unsaturated carboxylic acid derivative of the component (B) is selected from the group consisting of maleic acid monoesters, maleic acid diesters, maleic acid anhydride, itaconic acid monoesters, itaconic acid diesters, itaconic acid anhydride, fumaric acid monoesters, fumaric acid diesters, fumaric acid anhydride, alkyl acrylates, and alkyl methacrylates.

18. The method according to claim 17, wherein: The component (a1) is a copolymer of a cyclic olefin and an α-olefin having 2 to 8 carbon atoms, The amount of the structural unit derived from the cyclic olefin is 50% by mass or more.

19. The method according to claim 17, wherein: The component (a2) is a hydrogenated product of a random copolymer of an aromatic vinyl compound and a conjugated diene compound (a2-2).

20. A method for producing an adhesive coating, comprising: A step (1) of producing a thermoplastic resin composition by the method according to any one of claims 17 to 19; and and (2) dissolving the thermoplastic resin composition obtained in the step (1) in a solvent.

21. A method for manufacturing an extruded packaging product, comprising: A step (1) of producing a thermoplastic resin composition by the method according to any one of claims 17 to 19; a step of producing a laminate using the thermoplastic resin composition obtained in the step (1); and A process for producing an extrusion-packed product using the laminate obtained in the above process.