A composite material nanofiber and its preparation and application

By introducing composite nanofibers of rare earth oxide matrix and transition metal nanoparticles into water treatment materials, the problems of slow adsorption speed and poor circulation performance are solved, and rapid adsorption and stability of various organic pollutants are achieved, which is suitable for Sewage treatment and water purification installations.

CN109731543BActive Publication Date: 2024-10-29TSINGHUA UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910036440.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-01-15
Publication Date
2024-10-29
Estimated Expiration
2039-01-15

AI Technical Summary

Technical Problem

Existing water treatment materials have problems such as slow adsorption speed, high energy consumption in the regeneration process, and poor cycle performance. Moreover, the non-negligible secondary water pollution problem caused by chemically modified activated carbon materials has not been effectively solved.

Method used

Develop a composite nanofiber, which contains a rare earth oxide matrix and transition metal nanoparticles. It is prepared by electrospinning and heat treatment to prepare a nanofiber filter membrane for water treatment, which has the characteristics of rapid adsorption and multiple recycling.

Benefits of technology

It achieves rapid adsorption and stability of a variety of refractory organic pollutants, reduces water treatment costs, avoids secondary water pollution, and is suitable for sewage treatment and indoor and outdoor water purification devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109731543B_ABST
    Figure CN109731543B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite material nanofiber and its preparation and application. In particular, it relates to water purification treatment for organic micropollutants that are difficult to degrade in water bodies. The nanocomposite material provided by the present invention comprises a rare earth oxide matrix and metal nanoparticles dispersed in the interior and surface of the matrix, wherein the matrix is ​​a rare earth oxide of at least one rare earth element selected from Ce, Pr, Nd, Sm, Gd, Dy, Ho, Er, and Yb; and the metal nanoparticles are transition metals such as nickel, iron, cobalt, and copper. The present invention combines the triple effects of transition metal nanoparticles, rare earth oxides, and interface effects to obtain a nanocomposite material with an ultra-fast pollutant treatment effect, which can be widely used in various difficult-to-degrade water pollutants derived from industrial, agricultural, and medical industries. The material provided by the present invention has a simple preparation method, no secondary pollution, can be reused many times, reduces the cost of water treatment, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite material nanofiber and preparation and application thereof, and in particular to water treatment for difficult-to-degrade high-risk organic micropollutants in water bodies. Background Art

[0002] Adequate and safe water supply is the fundamental requirement for the operation of life and the basic condition for maintaining the sustainable development of industry and agriculture. However, water pollution caused by various pollutants has caused extremely serious water shortages in the world and endangered the safety of humans and other organisms. For example, a series of endocrine disruptors represented by bisphenol A and ethinyl estradiol, which are common in the water environment, are highly toxic at low concentrations and can have a huge impact on the endocrine system, ultimately leading to reproductive disorders, abnormal behavior, decreased reproductive capacity, juvenile death, and even extinction in animals and humans. In such a severe world water environment, it is crucial to develop efficient and multifunctional water purification materials. Using efficient and multifunctional water purification materials as filter membranes in portable indoor and outdoor water purification devices will also improve the safety factor of human drinking water.

[0003] At present, the research and development of adsorption materials is mostly focused on the surface modification of activated carbon materials, and considerable research results have been achieved. For example, the Chinese invention patent application with application number CN201710655860.2 and publication number CN107265529A discloses a multi-effect water treatment agent. It provides a method for grafting graphene oxide with acrylamide oligomers to prepare a water treatment agent material that can effectively remove benzene compounds.

[0004] The Chinese invention patent application with application number CN201610655714.5 and publication number CN106336239A discloses a new type of water treatment material. The method uses activated carbon, shale powder, tourmaline powder, etc. as raw materials to prepare microporous sewage filtration materials. However, there are still problems such as insufficient water treatment materials and low efficiency.

[0005] The above studies mainly use activated carbon as the matrix material for chemical modification or multi-phase composite. However, activated carbon materials have the defects of slow adsorption treatment speed, high energy consumption in the regeneration process and poor cycle performance. Furthermore, chemically modified activated carbon materials will bring about the problem of secondary water pollution that cannot be ignored, and the applicant has not evaluated this and proposed a solution. Therefore, the development of a new adsorption material with multiple effects, fast and excellent cycle performance will show great practical application value in the field of water treatment. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a composite material nanofiber and its preparation and application, which has the characteristics of wide application range, fast adsorption speed and excellent circulation performance. It also provides a new portable indoor and outdoor water treatment equipment based on the filter membrane prepared by the material.

[0007] In order to achieve the object of the present invention, the present invention provides a composite material nanofiber, wherein the composite material nanofiber comprises a rare earth oxide matrix and transition metal nanoparticles. Optionally, the composite material nanofiber consists of a rare earth oxide matrix and transition metal nanoparticles.

[0008] In the composite nanofiber provided by the present invention, the transition metal in the transition metal nanoparticles is selected from one or more of Ni, Co, Cu, Fe, Zn and Mn;

[0009] In the composite nanofiber provided by the present invention, the rare earth element in the rare earth metal oxide matrix is ​​selected from one or more of Ce, Pr, Nd, Sm, Gd, Dy, Ho, Er and Yb.

[0010] In the composite nanofiber provided by the present invention, the nanofiber diameter is 100nm-1000nm, and the transition metal nanoparticle size is 5nm-100nm;

[0011] In the composite nanofiber provided by the present invention, the rare earth oxide matrix accounts for 70-99wt.% of the composite nanofiber, and the transition metal nanoparticles account for 1-30wt.% of the composite nanofiber.

[0012] In the method for preparing the composite nanofiber provided by the present invention, optionally, in the composite nanofiber, the atomic ratio of transition metal to rare earth metal is 5-50 at.%, and the atomic percentage of rare earth metal is 95-50 at.%.

[0013] In the composite material nanofiber provided by the present invention, the composite material nanofiber is obtained by mixing rare earth metal nitrate and transition metal nitrate with a template agent, and then spinning and heat treating the mixture.

[0014] On the other hand, the present invention also provides a method for preparing composite nanofibers, comprising the following steps:

[0015] a) mixing a rare earth metal nitrate and a transition metal nitrate with a template in a solvent to prepare a precursor solution;

[0016] b) preparing a precursor fiber by spinning, wherein the spinning method is one of electrospinning, liquid spinning or gas spinning;

[0017] c) heat treating the precursor fiber in an inert atmosphere.

[0018] In the method for preparing the composite nanofiber provided by the present invention, optionally, the composite nanofiber is prepared by the above steps a), b) and c).

[0019] In the composite nanofiber or the method for preparing composite nanofiber provided by the present invention, the template agent is selected from one or more of polyvinyl alcohol PVA, polyvinyl butyral PVB, polyvinyl pyrrolidone PVP, polyvinylidene fluoride PVDF and polylactic acid PLA; the number average molecular weight Mn of the template agent is 10000-1300000;

[0020] In the method for preparing composite nanofibers provided by the present invention, the solvent in step a) is selected from one or more of water, ethanol, N,N-dimethylformamide DMF and acetic acid;

[0021] In the method for preparing composite nanofibers provided by the present invention, the mass ratio of the sum of the rare earth metal nitrate and the transition metal nitrate to the template agent is 1-10:2-15;

[0022] In the method for preparing composite nanofibers provided by the present invention, the mass ratio of the sum of the rare earth metal nitrate and the transition metal nitrate to the solvent is 1:1-1.5, and the optional mass ratio is 1:1-1.25;

[0023] In the method for preparing composite nanofibers provided by the present invention, the mass ratio of the rare earth metal nitrate to the transition metal nitrate is 2-25:1;

[0024] In the method for preparing composite nanofibers provided by the present invention, the precursor fiber heat treatment temperature in step c) is 700°C-1000°C, the heating rate is 4-10°C / min, and the heat treatment time is 1 h-5 h; the inert atmosphere gas is selected from one or more of inert gases and nitrogen.

[0025] In another aspect, the present invention provides a fiber filter membrane comprising the composite nanofibers described above. Optionally, the fiber filter membrane is composed of the composite nanofibers described above.

[0026] The fiber filter membrane provided by the present invention can be directly obtained through the process of preparing composite nanofibers, and the fiber filter membrane has a thickness of 0.5 mm to 20 mm;

[0027] Alternatively, the composite nanofibers are dispersed in a solvent by ultrasound, filtered, and dried. This method can be used to control the shape, thickness, and cross-sectional area of ​​the filter membrane. The thickness of the fiber filter membrane is 0.5 mm to 20 mm.

[0028] In the fiber filter membrane provided by the present invention, the mass ratio of the composite nanofiber to the solvent is 1-50:10-100; the solvent is selected from one or more of water, ethanol, methanol and polyvinylidene fluoride PVDF, and the ultrasonic frequency is 50-200 Hz.

[0029] On the other hand, the present invention provides one or more uses of fiber filter membranes for adsorbing impurities in water.

[0030] In the application of the fiber filter membrane provided by the present invention in adsorbing impurities in water, the fiber filter membrane is suitable for adsorbing common dyes such as rhodamine B, methylene blue, methyl blue, methyl orange and crystal violet; common pesticides such as pre-emergence herbicides Dole and Kindol; such as bisphenol A, bisphenol S, etc.; common industrial and manufacturing residues such as drugs; hormones such as ethinyl estradiol, heart disease drugs such as propranolol hydrochloride and beta-receptor blockers.

[0031] On the other hand, the present invention provides a water purification device, which comprises a fiber filter membrane, an organic polymer filter membrane and a packaging shell; optionally, the water purification device consists of a fiber filter membrane, an organic polymer filter membrane and a packaging shell.

[0032] In the water purification device provided by the present invention, the fiber filter membrane and the organic polymer filter membrane are alternately stacked at least once;

[0033] In the water purification device provided by the present invention, the alternating stacked structure of the fiber filter membrane and the organic polymer filter membrane is fixed by a packaging shell, and the packaging shell is provided with a water inlet and a water outlet. Water enters the packaging shell from the water inlet, passes through the alternating stacked structure composed of the fiber filter membrane and the organic polymer filter membrane, and then flows out from the water outlet.

[0034] In the water purification device provided by the present invention, the organic polymer filter membrane is selected from one or more of polyethylene membrane, polysulfone membrane, polyethersulfone membrane, polyamide membrane, cellulose membrane and polyvinylidene fluoride membrane.

[0035] In the water purification device provided by the present invention, the fiber filter membrane has a thickness of 0.5 mm-20 mm, and the organic polymer filter membrane has a thickness of 0.5 mm-20 mm; the alternating layers are stacked 2-20 times.

[0036] In the water purification device provided by the present invention, the packaging shell is a hollow cylinder with an inner diameter of 5mm-50mm and a height of 10mm-800mm.

[0037] The present invention adopts an innovative structural design. On the one hand, the adsorption material can quickly adsorb a variety of difficult-to-degrade organic pollutants in water, including dyes, pesticides, drugs and industrial residues; on the other hand, the adsorption material can be recycled multiple times, has stable performance and high commercial value.

[0038] The composite nanofiber adsorption material designed by the present invention has an exquisite structure design, simple preparation steps, low cost and mass production. The prepared composite nanofiber has a rapid and universal organic adsorption effect, is suitable for sewage treatment, outdoor survival, wartime and post-disaster drinking water supply, and has a very broad application prospect.

[0039] The advantages of the present invention are: firstly, a new type of rare earth metal oxide composite nanofiber adsorption material is designed; secondly, the prepared nanofiber can adsorb and remove a variety of difficult-to-degrade organic pollutants; thirdly, the prepared nanofiber has good stability and can maintain good adsorption performance during multiple cycles of use.

[0040] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The accompanying drawings are used to provide a further understanding of the technical solution of the present invention and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present invention and do not constitute a limitation on the technical solution of the present invention.

[0042] Figure 1 The electron microscope (SEM) photos of the novel multifunctional nanofiber materials with different nickel contents obtained in the examples of the present invention are shown in Figure 1. A. Sm2O3; B. 5 at. % Ni; C. 5.5 at. % Ni; D. 7 at. % Ni; E. 10 at. % Ni; F. 20 at. % Ni. Scale bar: 1 μm.

[0043] Figure 2 The X-ray diffraction results (XRD) of the multifunctional nanofiber materials based on different rare earth oxides obtained in the examples of the present invention.

[0044] Figure 3 The transmission electron microscope (TEM) photograph and energy spectrum distribution scanning result of the novel multifunctional nanofiber material obtained in Example 1 of the present invention are shown.

[0045] Figure 4Schematic diagram of the pollutant adsorption effect of the new multifunctional nanofiber material obtained in Example 31 of the present invention.

[0046] Figure 5 This is a schematic diagram of the cyclic performance of the new multifunctional nanofiber material obtained in Example 32 of the present invention.

[0047] Figure 6 This is a top view of a single-layer fiber filter membrane and polyethersulfone stacked together. The black part is the fiber filter membrane, and the layer below is the polyethersulfone membrane. The radius of the two membranes is set differently, the black fiber membrane is smaller, and the white part is the polyethersulfone membrane.

[0048] Figure 7 The cross-sectional view of the composite filter unit after packaging, wherein: 1-polyethersulfone membrane, 2-fiber filter membrane, 3-packaging shell.

[0049] Figure 8 Schematic diagram of a filter for household water purification.

[0050] Fig. 9 This is a schematic diagram of a portable outdoor water purification filter, where 4 is the water purification outlet, 5 is the water purification device, and 6 is tap water. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and advantages of the present invention more clear, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.

[0052] The present invention introduces transition metal nanoparticles into a rare earth oxide matrix through an innovative structural design to obtain a nanofiber adsorption material. On the one hand, the adsorption material can quickly adsorb a variety of difficult-to-degrade organic pollutants in water, including dyes, pesticides, drugs and industrial residues; on the other hand, the adsorption material can be recycled multiple times, has stable performance, and has high commercial value.

[0053] The present invention designs a new type of rare earth metal oxide nanofiber adsorption material, and provides a simple, low-cost and mass-producible preparation method. The adsorption material can produce a highly efficient removal effect on low-concentration organic pollutants that are difficult to degrade and highly harmful in the water treatment process. Secondly, the adsorption material designed by the present invention is universal and can produce excellent adsorption effects on various types of pollutants. Furthermore, the new adsorption material designed by the present invention can be recycled many times and has good performance stability. Secondly, the fiber filter membrane made based on the material provided by the present invention can be composited with a variety of polymer membranes to make a multi-level filtration device, which is suitable for portable indoor and outdoor water purification devices and has broad commercial application prospects. The present invention is further described below based on specific embodiments.

[0054] In a specific embodiment, the specific steps of preparing the precursor fiber by electrospinning are: transferring the electrospinning precursor solution to a syringe pump, adjusting the syringe pump propulsion speed to 1 ml·h -1 , the voltage was set to 15 kV, and the electrode distance was 20 cm. After continuous electrospinning, uniform precursor fibers were obtained on the collecting device.

[0055] Example 1

[0056] 1. Preparation of electrospinning precursor solution. 0.0343g of nickel nitrate and 0.7657g of samarium nitrate were dissolved in a mixture of 5g / 5g water and ethanol, so that the atomic percentage of nickel was 5at.%, and the atomic percentage of samarium was 95at.% based on the final product, and then polyvinylpyrrolidone (PVP, Mn1300000) was added at a final concentration of 8wt.%, so that the mass ratio of nitrate to PVP was 1:1; stirred at room temperature for 6 hours until the polyvinylpyrrolidone was completely dissolved and a uniform, transparent precursor solution with a certain fluidity was obtained.

[0057] 2. Preparation of precursor fibers by electrospinning.

[0058] 3. Heat treatment process. The collected precursor fibers are placed in a tube furnace, inert protective gas nitrogen is introduced, heated to 800°C at a heating rate of 5°C / min, and heat treated at 800°C for 2 hours. The heat treatment process can remove the polymer in the precursor fibers and obtain Ni / Sm2O3 inorganic composite nanofibers with good crystallization. The diameter of the nanofibers is 200nm and the size of the transition metal nanoparticles is 15nm.

[0059] 4. Add Ni / Sm2O3 nanofibers to a Rhodamine B solution with a concentration of 0.1 mM and a fiber loading of 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of Rhodamine B using a UV spectrophotometer.

[0060] 5. Experimental results show that Ni / Sm2O3 nanofibers can adsorb 99% of Rhodamine B in the solution within 10 seconds.

[0061] Example 2

[0062] 1. Preparation of electrospinning precursor solution. 0.0375g of nickel nitrate and 0.7625g of samarium nitrate were dissolved in a mixture of 5g / 5g water and ethanol, so that the atomic percentage of nickel was 5.5at.%, and the atomic percentage of samarium was 94.5at.%, and then polyvinylpyrrolidone (PVP, Mn1300000) was added at a final concentration of 8wt.%, so that the mass ratio of nitrate to PVP was 1:1; the mixture was stirred at room temperature for 6 hours until the polyvinylpyrrolidone was completely dissolved and a uniform, transparent precursor solution with a certain fluidity was obtained.

[0063] 2. Preparation of precursor fibers by electrospinning.

[0064] 3. Heat treatment process. The collected precursor fibers are placed in a tubular furnace, inert protective gas nitrogen is introduced, heated to 800°C at a heating rate of 5°C / min, and heat treated at 800°C for 2 hours. The heat treatment process can remove the polymer in the precursor fibers and obtain well-crystalline Ni / Sm2O3 inorganic composite nanofibers, with a nanofiber diameter of 180nm and a transition metal nanoparticle size of 10nm.

[0065] 4. Add Ni / Sm2O3 nanofibers to a Rhodamine B solution with a concentration of 0.1 mM and a fiber loading of 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of Rhodamine B using a UV spectrophotometer.

[0066] 5. Experimental results show that Ni / Sm2O3 nanofibers can adsorb 99% of Rhodamine B in the solution within 10 seconds.

[0067] Example 3

[0068] 0.0472g of nickel nitrate and 0.7528g of samarium nitrate were dissolved in a mixture of 5g / 5g of water and ethanol, so that the atomic percentage of nickel was 7at.%, and the atomic percentage of samarium was 93at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 220nm, and the size of the transition metal nanoparticles was 20nm.

[0069] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 10 seconds.

[0070] Example 4

[0071] 0.0657 g of nickel nitrate and 0.7343 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 250 nm, and the size of the transition metal nanoparticles was 40 nm.

[0072] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 97% of Rhodamine B in the solution within 10 seconds.

[0073] Example 5

[0074] 0.2472 g of nickel nitrate and 0.5528 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 30 at.%, and the atomic percentage of samarium was 70 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 300 nm, and the transition metal nanoparticle size was 60 nm.

[0075] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 95% of Rhodamine B in the solution within 10 seconds.

[0076] Example 6

[0077] The only difference between Example 6 and Example 2 is that the mass ratio of nitrate (rare earth metal nitrate and transition metal nitrate) to PVP is 0.8:1, and the final concentration of PVP is 10wt.%, thereby obtaining Ni / Sm2O3 inorganic composite nanofibers with good crystallization, a nanofiber diameter of 270nm, and a transition metal nanoparticle size of 25nm.

[0078] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 10 seconds.

[0079] Example 7

[0080] The only difference between Example 7 and Example 2 is that the mass ratio of nitrate (rare earth metal nitrate and transition metal nitrate) to PVB is 1:1, that is, polyvinyl butyral (PVB, Mn25000) with a final concentration of 8wt.% is used to obtain Ni / Sm2O3 inorganic composite nanofibers with good crystallization, the nanofiber diameter is 200nm, and the transition metal nanoparticle size is 20nm.

[0081] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 97% of Rhodamine B in the solution within 10 seconds.

[0082] Example 8

[0083] The only difference between Example 8 and Example 2 is that the mass ratio of nitrate (rare earth metal nitrate and transition metal nitrate) to PVA is 1:1, that is, polyvinyl alcohol (PVA, Mn66000) with a final concentration of 8wt.% is used to obtain Ni / Sm2O3 inorganic composite nanofibers with good crystallization, the nanofiber diameter is 200nm, and the transition metal nanoparticle size is 20nm.

[0084] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 97% of Rhodamine B in the solution within 10 seconds.

[0085] Example 9

[0086] The only difference between Example 9 and Example 2 is that the solvent used in the preparation of the electrospinning precursor solution is 9g N,N-dimethylformamide DMF, and well-crystalline Ni / Sm2O3 inorganic composite nanofibers are obtained. The nanofiber diameter is 200nm, and the transition metal nanoparticle size is 20nm.

[0087] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 97% of Rhodamine B in the solution within 10 seconds.

[0088] Example 10

[0089] 0.0554 g of nickel nitrate and 0.7446 g of cerium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of cerium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / CeO2 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 180 nm, and the transition metal nanoparticle size was 10 nm.

[0090] The test method is the same as that of Example 2. The experimental results show that Ni / CeO2 nanofibers can absorb 89% of Rhodamine B in the solution within 10 seconds.

[0091] Embodiment 11

[0092] 0.0713 g of nickel nitrate and 0.7287 g of neodymium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of neodymium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Nd2O3 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 220 nm, and the transition metal nanoparticle size was 50 nm.

[0093] The test method is the same as that of Example 2. The experimental results show that Ni / Nd2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 10 seconds.

[0094] Example 12

[0095] 0.0553 g of nickel nitrate and 0.7446 g of praseodymium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of praseodymium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Pr2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 210 nm, and the size of the transition metal nanoparticles was 40 nm.

[0096] The test method is the same as that of Example 2. The experimental results show that Ni / Pr2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 30 seconds.

[0097] Example 13

[0098] 0.0597g ​​of nickel nitrate and 0.7403g of gadolinium nitrate were dissolved in a mixture of 5g / 5g of water and ethanol, so that the atomic percentage of nickel was 10at.%, and the atomic percentage of gadolinium was 90at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Gd2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 230nm, and the size of the transition metal nanoparticles was 60nm.

[0099] The test method is the same as that of Example 2. The experimental results show that Ni / Gd2O3 nanofibers can absorb 93% of Rhodamine B in the solution within 30 seconds.

[0100] Embodiment 14

[0101] 0.0549 g of nickel nitrate and 0.7451 g of dysprosium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of dysprosium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Dy2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 250 nm, and the size of the transition metal nanoparticles was 70 nm.

[0102] The test method is the same as that of Example 2. The experimental results show that Ni / Dy2O3 nanofibers can absorb 95% of Rhodamine B in the solution within 60 seconds.

[0103] Embodiment 15

[0104] 0.0740 g of nickel nitrate and 0.7260 g of holmium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of holmium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Ho2O3 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 230 nm, and the transition metal nanoparticle size was 60 nm.

[0105] The test method is the same as that of Example 2. The experimental results show that Ni / Ho2O3 nanofibers can absorb 94% of rhodamine B in the solution within 40 seconds.

[0106] Example 16

[0107] 0.0679 g of nickel nitrate and 0.7321 g of ytterbium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of ytterbium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Yb2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 230 nm, and the size of the transition metal nanoparticles was 35 nm.

[0108] The test method is the same as that of Example 2. The experimental results show that Ni / Yb2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 40 seconds.

[0109] Embodiment 17

[0110] 0.0671 g of nickel nitrate and 0.7329 g of erbium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of nickel was 10 at.%, and the atomic percentage of erbium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Ni / Er2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 260 nm, and the size of the transition metal nanoparticles was 60 nm.

[0111] The test method is the same as that of Example 2. The experimental results show that Ni / Er2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 40 seconds.

[0112] Embodiment 18

[0113] 0.0724 g of cobalt nitrate and 0.7276 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of cobalt was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Co / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 310 nm, and the transition metal nanoparticle size was 40 nm.

[0114] The test method is the same as that of Example 2. The experimental results show that Co / Sm2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 20 seconds.

[0115] Embodiment 19

[0116] 0.0730 g of zinc nitrate and 0.7270 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of zinc was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. A well-crystallized Zn / Sm2O3 inorganic composite nanofiber was obtained, the nanofiber diameter was 210 nm, and the transition metal nanoparticle size was 60 nm.

[0117] The test method is the same as that of Example 2. The experimental results show that Zn / Sm2O3 nanofibers can absorb 96% of Rhodamine B in the solution within 10 seconds.

[0118] Embodiment 20

[0119] 0.0971 g of ferric nitrate and 0.7029 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of iron in the final product was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Fe / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the nanofiber diameter was 200 nm, and the transition metal nanoparticle size was 40 nm.

[0120] The test method is the same as that of Example 2. The experimental results show that Fe / Sm2O3 nanofibers can absorb 82% of Rhodamine B in the solution within 30 seconds.

[0121] Embodiment 21

[0122] 0.0763 g of copper nitrate and 0.7237 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of copper was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Cu / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 210 nm, and the size of the transition metal nanoparticles was 40 nm.

[0123] The test method is the same as that of Example 2. The experimental results show that the Cu / Sm2O3 nanofibers can adsorb 86% of the rhodamine B in the solution within 30 seconds.

[0124] Embodiment 22

[0125] 0.0896 g of manganese nitrate and 0.7104 g of samarium nitrate were dissolved in a mixture of 5 g / 5 g of water and ethanol, so that the atomic percentage of manganese was 10 at.%, and the atomic percentage of samarium was 90 at.%, and the remaining preparation conditions were the same as those in Example 2. Mn / Sm2O3 inorganic composite nanofibers with good crystallization were obtained, the diameter of the nanofibers was 230 nm, and the size of the transition metal nanoparticles was 30 nm.

[0126] The test method is the same as that of Example 2. The experimental results show that the Mn / Sm2O3 nanofibers can absorb 92% of the rhodamine B in the solution within 30 seconds.

[0127] Embodiment 23

[0128] The only difference between Example 23 and Example 2 is that during the heat treatment process, the inert atmosphere gas used is argon, and well-crystallized Ni / Sm2O3 inorganic composite nanofibers are obtained. The nanofiber diameter is 190nm, and the transition metal nanoparticle size is 15nm.

[0129] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 99% of Rhodamine B in the solution within 10 seconds.

[0130] Embodiment 24

[0131] The only difference between Example 24 and Example 2 is that during the heat treatment process, the inert atmosphere gas used is helium, and well-crystallized Ni / Sm2O3 inorganic composite nanofibers are obtained. The nanofiber diameter is 180nm, and the transition metal nanoparticle size is 10nm.

[0132] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 99% of Rhodamine B in the solution within 10 seconds.

[0133] Embodiment 25

[0134] The difference between Example 25 and Example 2 is that during the heat treatment process, the temperature is increased to 850°C at a rate of 5°C / min and the heat treatment is performed at 850°C for 2 hours. A Ni / Sm2O3 inorganic composite nanofiber with good crystallization is obtained. The diameter of the nanofiber is 300nm, and the size of the transition metal nanoparticle is 55nm.

[0135] The test method is the same as that of Example 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 98% of Rhodamine B in the solution within 10 seconds.

[0136] Embodiment 26

[0137] 1. Add the Ni / Sm2O3 nanofibers obtained in Example 2 to a bisphenol A solution, wherein the concentration of the bisphenol A solution is 0.1 mM and the fiber loading is 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of bisphenol A therein by using an ultraviolet spectrophotometer.

[0138] 2. Experimental results show that Ni / Sm2O3 nanofibers can absorb 90% of bisphenol A in the solution within 10 seconds.

[0139] Embodiment 27

[0140] 1. The Ni / Sm2O3 nanofibers obtained in Example 2 were added to a Dole solution (pre-emergence herbicide isopropylamine), the concentration of the Dole solution was 0.1 mM, and the fiber loading was 1 g / L. 1 ml of the solution was taken out at regular intervals, and the residual concentration of Dole therein was tested by a UV spectrophotometer.

[0141] 2. The experimental results show that Ni / Sm2O3 nanofibers can absorb 95% of Dole in the solution within 10 seconds.

[0142] Embodiment 28

[0143] 1. The Ni / Sm2O3 nanofibers obtained in Example 2 were added to an ethinyl estradiol solution, wherein the concentration of the ethinyl estradiol solution was 0.04 mM and the fiber loading was 1 g / L. 1 ml of the solution was taken out at regular intervals and the residual concentration of ethinyl estradiol therein was tested by a UV spectrophotometer.

[0144] 2. Experimental results show that Ni / Sm2O3 nanofibers can absorb 98% of ethinyl estradiol in the solution within 10 seconds.

[0145] Embodiment 29

[0146] 1. Add the Ni / Sm2O3 nanofibers obtained in Example 2 to a bisphenol S solution, wherein the concentration of the bisphenol S solution is 0.1 mM and the fiber loading is 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of bisphenol S therein by using an ultraviolet spectrophotometer.

[0147] 2. Experimental results show that Ni / Sm2O3 nanofibers can absorb 98% of bisphenol S in the solution within 10 seconds.

[0148] Embodiment 30

[0149] 1. The Ni / Sm2O3 nanofibers obtained in Example 2 were added to a mixed solution of bisphenol A, ethinyl estradiol, isopropyl metolachlor and bisphenol S, wherein the concentration of the ethinyl estradiol solution was 0.04 mM; the concentrations of bisphenol A, isopropyl metolachlor and bisphenol S were all 0.1 mM. The fiber loading was 1 g / L. 1 ml of the solution was taken out at intervals, and the residual concentration of each organic matter therein was tested by a UV spectrophotometer.

[0150] 2. Experimental results show that Ni / Sm2O3 nanofibers can absorb 98% of ethinyl estradiol, 86% of bisphenol A, 70% of isopropylamine and 90% of bisphenol S in the solution within 60 seconds.

[0151] Embodiment 31

[0152] 1. The Ni / Sm2O3 nanofibers obtained in Example 2 were added to a mixed solution of rhodamine B, methylene blue, and crystal violet, each with a concentration of 0.1 mM. The fiber loading was 1 g / L. 1 ml of the solution was taken out at regular intervals, and the residual concentration of each organic matter therein was tested by a UV spectrophotometer.

[0153] 2. Experimental results show that Ni / Sm2O3 nanofibers can absorb 98% of bisphenol A, 99% of methylene blue, and 97% of crystal violet in the solution within 60 seconds.

[0154] Embodiment 32

[0155] 1. Add the Ni / Sm2O3 nanofibers obtained in Example 2 to a bisphenol A solution, wherein the concentration of the bisphenol A solution is 0.1 mM and the fiber loading is 1 g / L. Centrifuge after reaching adsorption equilibrium and test the bisphenol A concentration in the clear solution.

[0156] 2. After separating the clear liquid, rinse the Ni / Sm2O3 nanofibers with ethanol to desorb bisphenol A.

[0157] 3. After rinsing with ethanol several times, wash with clean water, dry the nanofiber powder, and repeat steps 4 and 5 several times.

[0158] 4. Experimental results show that Ni / Sm2O3 nanofibers can maintain stable performance in 8 cycle tests and remove more than 95% of bisphenol A within 10 seconds.

[0159] Embodiment 33

[0160] 1. Preparation of liquid spinning precursor solution: 0.0343 g of nickel nitrate and 0.7657 g of samarium nitrate were dissolved in 10 g of a 1.0% aqueous solution of sodium dodecyl sulfate, so that the atomic percentage of nickel was 5 at.%, and the atomic percentage of samarium was 95 at.% based on the final product.

[0161] 2. Transfer the precursor solution to the syringe pump at a rate of 1 ml h -1 The Ni / Sm2O3 precursor fibers were then injected into a 15% by mass PVA solution (coagulation bath) at a speed of 1.5 %. The fibers were continuously drawn during continuous stirring to obtain Ni / Sm2O3 precursor fibers.

[0162] 3. Heat treatment process. The collected precursor fibers are placed in a tube furnace, inert protective gas helium is introduced, heated to 800°C at a heating rate of 5°C / min, and heat treated at 800°C for 2 hours. The heat treatment process can remove the polymer in the precursor fibers and obtain Ni / Sm2O3 inorganic composite nanofibers with good crystallization. The diameter of the nanofibers is 220nm, and the size of the transition metal nanoparticles is 30nm.

[0163] 4. Add the obtained Ni / Sm2O3 nanofibers to a bisphenol S solution with a concentration of 0.1 mM and a fiber loading of 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of bisphenol S therein by a UV spectrophotometer.

[0164] 5. Experimental results show that Ni / Sm2O3 nanofibers can absorb 95% of bisphenol S in the solution within 10 seconds.

[0165] Embodiment 34

[0166] 1. Preparation of vapor spinning precursor solution. 0.0343 g of nickel nitrate and 0.7657 g of samarium nitrate were dissolved in a mixture of 5 g of water and 5 g of ethanol, so that the atomic percentage of nickel was 5 at.%, and the atomic percentage of samarium was 95 at.% based on the final product. Then, polyvinyl pyrrolidone (PVP, Mn1300000) was added at a final concentration of 15 wt.%, and stirred at room temperature for 6 hours until the polyvinyl pyrrolidone was completely dissolved to obtain a uniform, transparent precursor solution with a certain fluidity.

[0167] 2. Transfer the precursor solution to the syringe pump at a rate of 5 ml h -1 The injection rate was up to 200 ml / min. -1 In an argon gas flow, Ni / Sm2O3 precursor fibers can be obtained at a receiving plate (which can be made of any material such as paper, plastic plate, aluminum foil, etc.) at a distance of 30 cm.

[0168] 3. Heat treatment process. The collected precursor fibers are transferred from the receiving plate to a crucible and placed in a tube furnace. Inert protective gas helium is introduced, heated to 800°C at a heating rate of 5°C / min, and heat treated at 800°C for 2 hours. The heat treatment process can remove the polymer in the precursor fibers and obtain Ni / Sm2O3 inorganic composite nanofibers with good crystallization. The nanofiber diameter is 200nm and the transition metal nanoparticle size is 20nm.

[0169] 4. Add the obtained Ni / Sm2O3 nanofibers to a bisphenol S solution with a concentration of 0.1 mM and a fiber loading of 1 g / L. Take out 1 ml of the solution at regular intervals and test the residual concentration of bisphenol S therein by a UV spectrophotometer.

[0170] 5. Experimental results show that Ni / Sm2O3 nanofibers can absorb 96% of bisphenol S in the solution within 10 seconds.

[0171] Embodiment 35

[0172] 1. 0.1 g of Ni / Sm2O3 nanofibers obtained in Example 2 were dispersed in 100 ml of deionized water by ultrasonic method, filtered to form a fiber filter membrane, and then dried in an oven. The fiber filter membrane had a thickness of 0.5 mm and a film cross-section of 20 mm. 2 .

[0173] 2. The above fiber filter membrane and polyethersulfone membrane are alternately assembled and stacked 20 times. The polyethersulfone membrane and the above fiber filter membrane have different hydrophilic and hydrophobic properties. The polyethersulfone membrane is 0.5 mm thick and is encapsulated in a 30 mm high plastic tube encapsulation shell to obtain a water purification device. One end of the water purification device can be processed with threads and connected by a pipeline, such as Figure 7 shown.

[0174] 3. The above-mentioned water purification device can be directly connected to the tap water pipeline. The tap water enters the water purification device through one end of the packaging shell encapsulating the fiber filter membrane and the polyethersulfone membrane, and flows out through the other end of the water purification device after being filtered by the fiber filter membrane and the polyethersulfone membrane, so as to conveniently purify the drinking water.

[0175] Embodiment 36

[0176] 1. 1 g of Ni / Sm2O3 nanofibers obtained in Example 12 were dispersed in 1000 ml of deionized water by ultrasonic method, filtered to form a fiber filter membrane, and then dried in an oven. The fiber filter membrane had a thickness of 1 mm and a cross-section of 20 mm. 2 .

[0177] 2. The above fiber filter membrane and polyethersulfone membrane are alternately assembled and stacked 15 times. The polyethersulfone membrane and the above fiber filter membrane have different hydrophilic and hydrophobic properties. The polyethersulfone membrane is 1 mm thick and is encapsulated in a 50 mm high plastic tube encapsulation shell to obtain a water purification device. One end of the water purification device can be processed with threads and connected by a pipeline, such as Figure 7 shown.

[0178] 3. Connect the above device directly to the tap water pipeline, and the tap water enters the water purification device through one end of the packaging shell encapsulated with the fiber filter membrane and the polyethersulfone membrane, and flows out through the other end of the water purification device after being filtered by the fiber filter membrane and the polyethersulfone membrane, so as to conveniently purify drinking water. Figure 8 In the household water purification filter shown, tap water enters the filter from the left inlet, the water flows downward in the space inside the water purification filter housing outside the encapsulation housing of the water purification device, flows into the lower end of the water purification device, is filtered through the fiber filter membrane and the polyethersulfone membrane, flows out from the upper end of the water purification device, and the filtered water flows out from the right outlet.

[0179] Embodiment 37

[0180] 1. 1 g of Ni / Sm2O3 nanofibers obtained in Example 2 were dispersed in 1000 ml of deionized water by ultrasonic method, filtered to form a fiber filter membrane, and then dried in an oven. The fiber filter membrane had a thickness of 1 mm and a cross-section of 20 mm. 2 .

[0181] 2. Alternately assemble and stack the above-mentioned fiber filter membrane and polymer membrane 16 times. The polymer membrane is a polyethylene membrane with different hydrophilic and hydrophobic properties from the above-mentioned film. The polyethylene membrane is 1.5 mm thick and is encapsulated in a 60 mm high plastic tube packaging shell to obtain a water purification device. One end of the water purification device can be processed into a straw (i.e., the purified water outlet) and a porous plug is installed at the other end.

[0182] 3. For example Fig. 9 As shown, the above-mentioned water purification device is directly installed in a water cup. Water enters the water purification device through the porous plug at one end of the water purification device, namely the water inlet of the water purification device, and flows out through the water outlet after being filtered by the fiber filter membrane and the polyethylene membrane. Bacteria, parasites and impurities in the water can be removed, and drinking water purification in the wild, post-disaster areas and other areas can be conveniently realized.

[0183] Although the embodiments disclosed in the present invention are as above, the contents described are only embodiments adopted to facilitate understanding of the present invention and are not intended to limit the present invention. Any technician in the field to which the present invention belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present invention, but the patent protection scope of the present invention shall still be defined by the attached claims.

Claims

1. A composite nanofiber adsorption material for use in adsorbing organic pollutants in water, wherein the composite nanofiber adsorption material comprises a rare earth oxide matrix and transition metal nanoparticles, in, The metal element in the transition metal nanoparticles is selected from one or more of Ni, Co, Cu, Fe, Zn and Mn; The rare earth element in the rare earth oxide matrix is ​​selected from one or more of Ce, Pr, Nd, Sm, Gd, Dy, Ho, Er and Yb, Wherein, the rare earth oxide matrix accounts for 70-99wt.% of the nanofiber adsorption material, and the transition metal nanoparticles account for 1-30wt.% of the nanofiber adsorption material; In the composite nanofiber adsorption material, the atomic ratio of transition metal to rare earth metal is 5-50 at.%, and the atomic percentage of rare earth metal is 95-50 at.%.

2. The use according to claim 1, wherein The diameter of the nanofiber adsorption material is 100nm-1000nm, and the size of the transition metal nanoparticles is 5nm-100nm.

3. The use according to claim 1, wherein The composite material nanofiber adsorption material is prepared by mixing rare earth metal nitrate and transition metal nitrate with a template agent, and then spinning and heat treating the mixture to obtain the composite material nanofiber adsorption material.

4. The use according to any one of claims 1 to 3, wherein The composite nanofiber adsorption material is prepared by a method comprising the following steps: a) mixing a rare earth metal nitrate and a transition metal nitrate with a template in a solvent to prepare a precursor solution; b) preparing a precursor fiber by spinning, wherein the spinning method is one of electrospinning, liquid spinning or gas spinning; c) heat treating the precursor fiber in an inert atmosphere, Wherein, the solvent in step a) is selected from one or more of water, ethanol, N,N-dimethylformamide DMF and acetic acid; The mass ratio of the sum of the rare earth metal nitrate and the transition metal nitrate to the template is 1-10:1-15; the mass ratio of the sum of the rare earth metal nitrate and the transition metal nitrate to the solvent is 0.1:1-1.25; the mass ratio of the rare earth metal nitrate to the transition metal nitrate is 2-25:

1.

5. The use according to claim 4, wherein The template agent is selected from one or more of polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinyl pyrrolidone (PVP), polyvinylidene fluoride (PVDF) and polylactic acid (PLA); and the number average molecular weight (Mn) of the template agent is 10,000-1,300,000.

6. The use according to claim 4, wherein In step c), the precursor fiber heat treatment temperature is 700°C-1000°C, the heating rate is 4-10°C / min, and the heat treatment time is 1h-5h; the inert atmosphere gas is selected from one or more of inert gas and nitrogen.

7. Use of a fiber filter membrane in adsorbing organic pollutants in water, wherein: The fiber filter membrane comprises the composite nanofiber adsorption material described in any one of claims 1 to 3.

8. The use according to claim 7, wherein The fiber filter membrane is directly obtained in the process of preparing the composite nanofiber adsorption material, and the fiber filter membrane has a thickness of 0.5 mm to 20 mm; Alternatively, the composite nanofiber adsorbent material is prepared by ultrasonically dispersing the composite nanofiber adsorbent material in a solvent, filtering by suction, and drying; The mass ratio of the composite material nanofiber adsorption material to the solvent is 1-50:10-100; the solvent is selected from one or more of water, ethanol and methanol, and the ultrasonic frequency is 50-200 Hz.

9. A water purification device, characterized in that: Composed of the fiber filter membrane and the organic polymer filter membrane and a packaging shell in any one of claims 7 or 8; The fiber filter membrane and the organic polymer filter membrane are alternately stacked at least once; The fiber filter membrane and the organic polymer filter membrane have different hydrophilic and hydrophobic properties; The alternating stacked structure of the fiber filter membrane and the organic polymer filter membrane is fixed by a packaging shell, which is provided with a water inlet and a water outlet. Water enters the packaging shell from the water inlet, passes through the alternating stacked structure of the fiber filter membrane and the organic polymer filter membrane, and then flows out from the water outlet.

10. The water purification device according to claim 9, characterized in that: The organic polymer filter membrane is selected from one or more of a polyethylene membrane, a polysulfone membrane, a polyethersulfone membrane, a polyamide membrane, a cellulose membrane and a polyvinylidene fluoride membrane.

11. The water purification device according to claim 9 or 10, characterized in that: The fiber filter membrane has a thickness of 0.5 mm to 20 mm, and the organic polymer filter membrane has a thickness of 0.5 mm to 20 mm; the alternating layers are stacked 2 to 20 times.

12. The water purification device according to claim 9 or 10, characterized in that: The packaging shell is a hollow cylinder with an inner diameter of 5mm-50mm and a height of 10mm-800mm.

Citation Information

Patent Citations

  • Novel water treatment material preparation method

    CN106336239A

  • Multiple-effect water treatment agent, and preparation method and water treatment method thereof

    CN107265529A