Preparation method of diamond-coated metal mesh for oil-water separation, metal mesh coating deposition device, diamond-coated metal mesh and application thereof
Nanodiamonds are grown at low temperature on metal meshes through hot wire chemical vapor deposition technology, which solves the problems of high cost and short service life of oil-water separation metal meshes, achieves efficient and long-life oil-water separation effects, and is suitable for industrial production.
Patent Information
- Application Number
- CN201810202142.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-03-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2038-03-12
AI Technical Summary
The existing oil-water separation metal mesh has problems such as high cost, short service life, limited types of oil-water separation, and easy function failure. Moreover, the preparation method of the diamond coating is complicated and not suitable for industrial production.
Hot wire chemical vapor deposition technology is used to deposit a diamond coating on the surface of the metal mesh. Nanodiamonds are grown at low temperature to avoid deformation of the metal mesh. A simple deposition device is designed to fix the metal mesh to achieve three-dimensional diamond coating deposition.
A diamond-coated metal mesh with high oil-water separation efficiency and long service life is achieved, which is suitable for industrial production and large-scale applications, has low cost, and is suitable for diamond film deposition on large-size workpieces.
Smart Images

Figure CN110257799B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oil-water separation metal meshes, and in particular to a method for preparing an oil-water separation diamond-coated metal mesh, a metal mesh coating deposition device, a diamond-coated metal mesh and applications thereof. Background Art
[0002] Since the beginning of the new century, oil-water separation technology has been widely used in many fields such as petrochemicals, sewage treatment, and food engineering. At present, oily wastewater is mainly treated by gravity sedimentation, coarse granulation, centrifugal separation and other methods. Although these methods can treat oily wastewater, they have the disadvantages of low separation efficiency, high cost, and low recovery rate. Oil-water separation is an important industrial process for treating oily wastewater and water-containing oil. Oil-water separation is to separate oil from water by using the completely different wettability of the same material to oil and water, such as the material has super-hydrophobic and super-oleophilic properties or super-hydrophilic and super-oleophobic properties. Subsequently, the development and research of super-hydrophobic and super-oleophilic filter materials has gradually deepened, and these filter materials are oleophilic and hydrophobic. The general method is to modify the porous structure of the material to be super-hydrophobic, and among various porous structures, metal wire mesh has become an ideal material due to its low cost, high mechanical strength and porous structure.
[0003] Conventional metal mesh can be modified on the surface of the metal mesh structure by surface modification. The modification can be carried out by acid-base corrosion or by using a surface modifier. Typically, the surface structure is changed by corrosion to induce super-hydrophobic and super-oleophilic properties. For example, a metal copper mesh is corroded in a nitric acid solution to increase the roughness of the copper wire surface, and hexadecanethiol is modified to make it have super-hydrophobic and super-oleophilic properties. This method can achieve the effect of oil-water separation.
[0004] However, due to the differences in the state of oil-water mixing, oil-water content, types of organic matter contained in the oil-water mixture, oil-water separation objects and other factors, the difficulty of oil-water separation has become increasingly greater. At the same time, the surface modification of metal mesh to make it hydrophobic and oleophilic has also encountered many limitations in practical applications: first, the corrosion resistance of the metal mesh itself is limited, it is easily corroded by the environment, and its service life is short; second, the surface modification of the metal mesh is used in oil-water separation with strong specificity, and the types of oils are relatively small. Specific oil-water separation requires corresponding specific corrosion and modifier treatment; third, when oil-water separation is performed by acid-base corrosion or surface modifier modification, the time cannot be very long. The hydrophobic functional groups added to the metal surface by acid-base corrosion and adding surface modifiers are only on the surface and are prone to failure.
[0005] Some materials for oil-water separation have appeared in the prior art, such as patent CN106987876 A discloses a method for preparing a super-hydrophobic / oleophilic oil-water separation Ni-Cu composite coating mesh film, which first performs Ni-Cu composite electroplating on the metal surface to enhance the corrosion resistance of the metal, and then uses a low-energy surface modifier to surface modify the coating so that it obtains a hydrophilic / oleophobic function. The method is complex, requires two process treatments, and has a short service life. The low-energy active agent adsorbed on the metal surface is easily invalidated, resulting in the loss of hydrophilic / oleophobic function. Patent CN106362439A discloses a method for preparing an oil-water separation metal mesh with hydrophilic / underwater superoleophobicity. The patent uses a laser processing method to process a micro-nano structure on the metal surface, so that it has a hydrophilic and oleophobic effect, but the laser processing cost is extremely high, and it is easy to destroy the basic original phase structure.
[0006] At present, the main technical problems of metal mesh used in oil-water separation are high cost, short service life, limited types of oil-water separation and easy failure of function.
[0007] On the other hand, diamond is the hardest substance in the world, with extremely stable physical and chemical properties and a high elastic modulus. The prior art patent CN 103741116 A has proposed a method for growing a CVD diamond coating on a metal mesh substrate to make the surface of the diamond mesh super-hydrophobic and hydrophilic, but the process of this method is relatively complicated, the deposition equipment used is expensive and costly, and diamond films can only be grown on small-sized workpieces, which is not suitable for metal meshes for actual oil-water separation and is not conducive to industrial production and industrial use.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] One of the purposes of the present invention is to provide a method for preparing a diamond-coated metal mesh for oil-water separation, wherein a diamond coating is deposited on the surface of the metal mesh by hot wire chemical vapor deposition, the temperature used by the hot wire chemical vapor deposition method is usually lower than that of other methods, and the method of growing nanodiamonds at low temperature effectively avoids deformation of the metal mesh during the deposition process. The method has a fast film-forming rate, a simple preparation process, a stable process, and a low cost, and is suitable for industrial production and large-scale industrial use.
[0010] The second object of the present invention is to provide a metal mesh coating deposition device using hot wire chemical vapor deposition in the preparation method of the above-mentioned oil-water separation diamond coated metal mesh. The deposition device is simple and can fix the metal mesh. The metal mesh will not be deformed during the deposition process and is very suitable for the preparation of chemical vapor deposition coatings in three-dimensional directions.
[0011] The third object of the present invention is to provide a diamond coated metal mesh prepared by the preparation method of the above-mentioned oil-water separation diamond coated metal mesh or a diamond coated metal mesh obtained by hot wire chemical vapor deposition using the above-mentioned metal mesh coating deposition device, which has the advantages of high oil-water separation efficiency and long service life.
[0012] A fourth object of the present invention is to provide an application of the above-mentioned diamond-coated metal mesh in oil-water separation.
[0013] A fifth object of the present invention is to provide an oil-water separation device comprising the above-mentioned diamond-coated metal mesh.
[0014] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0015] In a first aspect, a method for preparing a diamond-coated metal mesh for oil-water separation is provided, comprising the following steps:
[0016] Depositing a diamond coating on the surface of the metal mesh by hot wire chemical vapor deposition to obtain a diamond coated metal mesh;
[0017] Preferably, the metal mesh is a copper mesh, a titanium mesh or a stainless steel mesh.
[0018] Preferably, on the basis of the technical solution of the present invention, during hot wire chemical vapor deposition, the gas source includes hydrogen and methane gas, and the temperature of the reaction zone is 500-800°C, preferably 500-700°C, and further preferably 500-600°C;
[0019] Preferably, the temperature of the reaction zone is increased from room temperature to 500-800°C at a heating rate of 15-25°C / min and maintained for 10-20 min.
[0020] Preferably, on the basis of the technical solution of the present invention, the gas source further includes an inert gas; the total flow rate of hydrogen, methane and inert gas during the reaction is 400-600 mL / min, preferably 400-500 mL / min, wherein the methane gas flow rate accounts for 1-5% of the total flow rate, the hydrogen flow rate accounts for 25-45% of the total flow rate, and the inert gas flow rate accounts for 50-70% of the total flow rate;
[0021] and / or, the deposition pressure is 1500-2000 Pa, preferably 1500-1800 Pa, further preferably 1500-1600 Pa;
[0022] and / or, the vertical distance between the upper row of heating wires and the metal mesh is 20-25 mm, and the vertical distance between the lower row of heating wires and the metal mesh is 15-20 mm;
[0023] And / or, the deposition time is 1.5-3 h, preferably 1.5-2.5 h, and further preferably 2-2.5 h.
[0024] Preferably, on the basis of the technical solution of the present invention, the metal mesh is a metal mesh that has been treated with nano-diamond crystallization;
[0025] Preferably, the crystal planting treatment includes placing the metal mesh in a crystal planting solution and ultrasonicating for 20-60 minutes, then taking it out and drying it, and the preferred drying method is to blow dry it with an inert gas;
[0026] Preferably, the planting solution is a nano-diamond suspension; the nano-diamond suspension preferably comprises nano-diamond powder, dimethyl carbonate and water, the mass of the nano-diamond powder accounts for 0.005-0.01% of the mass of the nano-diamond suspension, and the concentration of dimethyl carbonate in the nano-diamond suspension is 1×10 -6 -10×10 -6 mol / L; preferably the pH of the nanodiamond suspension is 2-4.
[0027] Preferably, based on the technical solution of the present invention, the method for preparing the oil-water separation diamond-coated metal mesh comprises the following steps:
[0028] (a) cleaning the surface of the metal mesh;
[0029] (b) performing corrosion treatment on the cleaned metal mesh;
[0030] (c) cleaning the metal mesh again;
[0031] (d) performing nano-diamond crystal planting treatment on the metal mesh;
[0032] (e) depositing a diamond coating on the surface of the metal mesh by hot wire chemical vapor deposition after the crystal planting process to obtain a diamond coated metal mesh;
[0033] Preferably, step (a) and step (c) independently include first ultrasonic cleaning with water for 2-3 times, each time for 5-10 minutes, and then ultrasonic cleaning with alcohol for 1-2 times, each time for 5-10 minutes;
[0034] Preferably, step (b) comprises first ultrasonicating in an alkaline solution for 5-10 min, and then ultrasonicating in an acid solution for 30-60 s; preferably, the alkaline solution is a 0.5-1 mol / L NaOH solution; preferably, the acid solution is a 0.5-1 mol / L HCl solution;
[0035] Preferably, step (d) comprises placing the metal mesh in a crystal planting solution and ultrasonicating for 20-60 minutes, then taking it out and drying it, and preferably drying it by blowing it with nitrogen; preferably, the crystal planting solution is a nano-diamond suspension; the nano-diamond suspension preferably comprises nano-diamond powder, dimethyl carbonate and water, the mass of the nano-diamond powder accounts for 0.005-0.01% of the mass of the nano-diamond suspension, and the concentration of dimethyl carbonate in the nano-diamond suspension is 1×10 -6 -10×10 -6 mol / L; preferably the pH of the nanodiamond suspension is 2-4.
[0036] In a second aspect, a metal mesh coating deposition device for hot wire chemical vapor deposition in the above-mentioned method for preparing the oil-water separation diamond-coated metal mesh is provided, wherein the metal mesh coating deposition device comprises a clamp body located between the upper and lower heat exhaust wires;
[0037] The clamp body comprises a first body and a second body arranged in parallel, the first body and the second body each independently have a hollow inside, a metal mesh is placed between the first body and the second body, and the edge size of the metal mesh is larger than the hollow size of the first body and the second body, and the first body and the second body are fixed by a detachable clamping mechanism perpendicular to the first body to clamp the metal mesh between the first body and the second body;
[0038] Preferably, both the first body and the second body are molybdenum disks;
[0039] Preferably, the detachable clamping mechanism comprises a bolt and a nut.
[0040] Preferably, based on the technical solution of the present invention, the clamp body further comprises a first spring sheet and / or a second spring sheet;
[0041] The first spring sheet is located inside the first body;
[0042] The second spring piece is located inside the second body.
[0043] In a third aspect, a diamond coated metal mesh prepared by the above-mentioned method for preparing the oil-water separation diamond coated metal mesh or a diamond coated metal mesh obtained by hot wire chemical vapor deposition using the above-mentioned metal mesh coating deposition device is provided.
[0044] In a fourth aspect, a use of the diamond-coated metal mesh in oil-water separation is provided.
[0045] Preferably, on the basis of the technical solution of the present invention, the diamond coated metal mesh is placed in an oil-water mixture, and the oil can pass through the diamond coated metal mesh but the water cannot pass through the diamond coated metal mesh, thereby achieving the purpose of oil-water separation.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] (1) The present invention is highly practical and uses hot wire chemical vapor deposition technology to deposit low-temperature nanodiamonds on a metal mesh. This method is applicable to the deposition of diamond coatings on any metal mesh and effectively avoids deformation of the metal mesh during the deposition process. The diamond deposition equipment of this method is simple, the film formation rate is fast, the operation is convenient, and the process is stable. The diamond film prepared on the metal mesh by the present invention is suitable for industrial mass production, has low cost, and can deposit a diamond coating with good bonding force on each surface of the metal mesh in three dimensions. This method can grow diamond films on large-sized workpieces and is suitable for large-scale industrial applications.
[0048] (2) The present invention uses the effect of hot wire chemical vapor deposition to grow a diamond coating on a metal mesh in three dimensions to obtain a diamond-coated metal mesh, which can be used for oil-water separation. Since diamond has extremely high physical and chemical stability, it can not only resist corrosion from strong acids and alkalis, but also its high hardness and elastic modulus can greatly increase its service life. Compared with other methods, the diamond-coated metal mesh prepared by this method has high oil-water separation efficiency and long service life.
[0049] (3) The present invention designs a fixture for metal mesh deposition and a device suitable for three-dimensional deposition of nanodiamond coating on the surface of the metal mesh. The designed hot wire chemical vapor deposition device has a simple structure and can fix the metal mesh. The metal mesh will not be deformed during the deposition process. The deposition temperature of the metal mesh is more uniform, and the diamond film on the metal mesh grows more uniformly. It is very suitable for the preparation of chemical vapor deposition coatings in three-dimensional directions. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 A top view of a metal mesh coating deposition device according to an embodiment of the present invention;
[0051] Figure 2 A front view of a metal mesh coating deposition device according to an embodiment of the present invention;
[0052] Figure 3 This is a surface morphology diagram of the metal mesh in Example 1 of the present invention;
[0053] Figure 4 This is a surface morphology of the diamond film grown on the metal mesh in Example 1 of the present invention.
[0054] Icons: 100 - clamp body; 110 - first body; 120 - second body; 130 - detachable clamping mechanism; 131 - bolt; 132 - nut; 141 - first spring sheet; 142 - second spring sheet; 200 - metal mesh; 300 - upper and lower heat discharge wires. DETAILED DESCRIPTION
[0055] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0056] According to a first aspect of the present invention, there is provided a method for preparing a diamond-coated metal mesh for oil-water separation, comprising the following steps:
[0057] A diamond coating is deposited on the surface of the metal mesh by hot wire chemical vapor deposition to obtain a diamond coated metal mesh.
[0058] Hot wire chemical vapor deposition (hot wire CVD) is a type of chemical vapor deposition method. This method mainly decomposes hydrocarbon gas to produce SP necessary for synthetic diamond. 3 Hybridized orbitals of carbon atoms.
[0059] There is no limitation on the hot wire chemical vapor deposition method, and conventional hot wire chemical vapor deposition equipment and / or processes may be used. It may be a common hot wire method or other improved forms of hot wire method such as electronic assistance.
[0060] Typical but non-limiting metal meshes are, for example, copper mesh, titanium mesh or stainless steel mesh.
[0061] Diamond is the hardest substance in the world, with extremely stable physical and chemical properties and a high elastic modulus. The three-dimensional nanodiamond coating is deposited on the surface of the metal mesh by hot wire chemical vapor deposition. During the deposition process, a carbon source and a hydrogen source are required. The carbon source provides the growth of diamond, and the hydrogen source generates active hydrogen groups -H to etch the SP in the non-diamond phase. 2 Bonds, so there will be a large number of -H group terminals in the entire deposition process, which are doped in the diamond coating as a whole. The -H terminals will create a special structure that is super hydrophobic, but not oleophobic. Hot wire-assisted chemical vapor deposition technology is used to directly deposit a hydrophobic and oleophilic nanodiamond coating on the surface of the metal mesh.
[0062] The temperature of the hot wire chemical vapor deposition method is usually lower than that of other methods (such as microwave method and flame combustion method). It is a method for growing nano diamonds at low temperature, which can effectively avoid deformation of the metal mesh during the deposition process. Compared with other methods, the method of the present invention has a fast film formation rate, simple deposition equipment, is suitable for large-area deposition, has a simple preparation process, a stable process, and low cost, and is suitable for industrial production and large-scale industrial use. By using the effect of hot wire chemical vapor deposition, a diamond coating is grown three-dimensionally (in all directions) on the metal mesh. The diamond-coated metal mesh prepared by this method is hydrophobic and oleophilic, and can be used in oil-water separation with high oil-water separation efficiency. Since diamond has extremely high physical and chemical stability, it can not only withstand corrosion from strong acids and alkalis, but also the high hardness and elastic modulus of diamond can greatly increase the service life of the metal mesh itself.
[0063] In a preferred embodiment, during hot wire chemical vapor deposition, the gas source includes hydrogen and methane, and the temperature of the reaction zone is 500-800°C, preferably 500-700°C, and further preferably 500-600°C.
[0064] During the deposition process, CH 4 and H 2 , where CH 4 Provides carbon source for diamond growth, H 2 Generate active hydrogen radicals -H to etch the non-diamond phase SP 2 key.
[0065] Typical but non-limiting reaction zone temperatures are, for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, or 800°C.
[0066] Preferably, the temperature of the reaction zone is increased from room temperature to 500-800°C at a heating rate of 15-25°C / min and maintained for 10-20 min.
[0067] Typical but non-limiting examples of the heating rate are 15°C / min, 20°C / min or 25°C / min.
[0068] Typical but non-limiting examples of incubation times are 10 min, 15 min or 20 min.
[0069] The temperature of the reaction zone is low during hot wire chemical vapor deposition, which alleviates the defect that the metal mesh is easily deformed during the deposition process, resulting in ineffective deposition.
[0070] In a preferred embodiment, the gas source also includes an inert gas; the total flow rate of hydrogen, methane gas and inert gas during the reaction is 400-600 mL / min, preferably 400-500 mL / min, wherein the methane gas flow rate accounts for 1-5% of the total flow rate, the hydrogen flow rate accounts for 25-45% of the total flow rate, and the inert gas flow rate accounts for 50-70% of the total flow rate.
[0071] A typical but non-limiting inert gas is argon.
[0072] The total flow rate of hydrogen gas, methane gas and inert gas is controlled to be, for example, 400 mL / min, 450 mL / min, 500 mL / min, 550 mL / min or 600 mL / min.
[0073] The methane gas flow accounts for 1-5% of the total flow, such as 1%, 2%, 3%, 4% or 5%, the hydrogen flow accounts for 25-45% of the total flow, such as 25%, 30%, 35%, 40% or 45%, and the inert gas flow accounts for 50-70% of the total flow, such as 50%, 55%, 60%, 65% or 70%.
[0074] By controlling the total flow rate and the flow ratio of hydrogen, methane and inert gas, a nanodiamond film with good quality and strong adhesion can be grown. Too little hydrogen is not conducive to the generation of active hydrogen radicals -H to etch the non-diamond phase SP 2 Key, CH 4 Too little gas cannot provide sufficient carbon source for diamond growth.
[0075] In a preferred embodiment, the deposition pressure is 1500-2000 Pa, preferably 1500-1800 Pa, and further preferably 1500-1600 Pa.
[0076] The deposition pressure is typically, but not limited to, 1500 Pa, 1600 Pa, 1700 Pa, 1800 Pa, 1900 Pa or 2000 Pa, for example.
[0077] By controlling the deposition pressure, it is beneficial to obtain a high-quality film layer, and the grown diamond film has a dense structure.
[0078] In a preferred embodiment, the vertical distance between the upper row of heating wires and the metal mesh is 20-25 mm, and the vertical distance between the lower row of heating wires and the metal mesh is 15-20 mm.
[0079] The distance between the upper row of hot wires and the sample is, for example, 20 mm, 21 mm, 22 mm, 23 mm, 24 mm or 25 mm; the distance between the lower row of hot wires and the sample is, for example, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm or 20 mm.
[0080] The deposition temperature of the metal mesh is ensured by controlling the distance between the upper and lower heat discharge wires and the sample, making the deposition temperature more suitable and uniform.
[0081] In a preferred embodiment, the deposition time is 1.5-3 h, preferably 1.5-2.5 h, and more preferably 2-2.5 h.
[0082] Typical but non-limiting deposition times are, for example, 1.5 h, 2 h, 2.5 h or 3 h.
[0083] By controlling the deposition time, the diamond film grown has an appropriate thickness and good adhesion.
[0084] In a preferred embodiment, the metal mesh is a metal mesh that has been treated with nano-diamond crystallization; that is, the metal mesh is treated with nano-diamond crystallization before a diamond coating is deposited on the surface of the metal mesh by hot wire chemical vapor deposition.
[0085] The crystal planting process is to pre-implant a layer of tiny diamond particles on the surface of the substrate as nucleation points to increase the diamond deposition density.
[0086] A typical but non-limiting method of the seeding treatment is to ultrasonically treat the substrate surface with a suspension containing diamond powder.
[0087] Preferably, the crystal planting treatment includes placing the metal mesh in a crystal planting solution, ultrasonicating for 20-60 minutes, and then taking it out to dry. The preferred drying method is to blow dry with an inert gas, preferably nitrogen.
[0088] The ultrasound time is typically, but not limited to, 20 min, 30 min, 40 min, 50 min or 60 min.
[0089] Preferably, the planting solution is a nano-diamond suspension; preferably, the nano-diamond suspension comprises nano-diamond powder, dimethyl carbonate and water, the mass of the nano-diamond powder accounts for 0.005-0.01% of the mass of the nano-diamond suspension, and the concentration of dimethyl carbonate in the nano-diamond suspension is 1×10 -6 -10×10 -6 mol / L; preferably the pH of the nanodiamond suspension is 2-4.
[0090] The nano-diamond suspension is nano-diamond powder dispersed in a solvent of dimethyl carbonate and water, and the mass fraction of the nano-diamond powder is 0.005-0.01%, such as 0.005%, 0.006%, 0.007%, 0.008%, 0.009% or 0.01%. The concentration of dimethyl carbonate (DMC) is 1×10 -6 mol / L、2×10 -6 mol / L、3×10 -6mol / L、4×10 -6 mol / L、5×10 - 6 mol / L、6×10 -6 mol / L、7×10 -6 mol / L、8×10 -6 mol / L、9×10 -6 mol / L or 10×10 -6 mol / L. The pH of the nanodiamond suspension is 2-4, such as pH2, pH3 or pH4.
[0091] After the metal mesh is subjected to a crystal planting treatment using the nano-diamond suspension (crystal planting solution), the diamond powder debris remaining in the surface defects of the metal mesh can provide nucleation cores for hot wire chemical vapor deposition of diamonds, thereby increasing the nucleation density and significantly improving the adhesion between the diamond film and the substrate.
[0092] In a preferred embodiment, the method for preparing the oil-water separation diamond-coated metal mesh comprises the following steps:
[0093] (a) cleaning the surface of the metal mesh;
[0094] (b) performing corrosion treatment on the cleaned metal mesh;
[0095] (c) cleaning the metal mesh again;
[0096] (d) performing nano-diamond crystal planting treatment on the metal mesh;
[0097] (e) depositing a diamond coating on the surface of the metal mesh by hot wire chemical vapor deposition after the crystal planting process to obtain a diamond coated metal mesh;
[0098] Preferably, step (a) comprises first ultrasonic cleaning with water for 2-3 times, each time for 5-10 minutes, and then ultrasonic cleaning with alcohol for 1-2 times, each time for 5-10 minutes.
[0099] First clean the surface of the metal mesh to remove impurities on the surface of the metal mesh and keep the surface of the sample clean.
[0100] Preferably, step (b) comprises first ultrasonicating in an alkaline solution for 5-10 min and then ultrasonicating in an acid solution for 30-60 s; preferably, the alkaline solution is a 0.5-1 mol / L NaOH solution; preferably, the acid solution is a 0.5-1 mol / L HCl solution.
[0101] First, ultrasonicate in the alkaline solution for 5-10 min, such as 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, and then ultrasonicate in the acid solution for 30-60 s, such as 30 s, 40 s, 50 s or 60 s.
[0102] The concentration of the alkaline solution is, for example, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L; the concentration of the acid solution is, for example, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L.
[0103] The cleaned metal mesh is corroded to increase the surface roughness and improve the adsorption density of diamond particles.
[0104] Preferably, step (c) comprises first ultrasonic cleaning with water for 2-3 times, each time for 5-10 minutes, and then ultrasonic cleaning with alcohol for 1-2 times, each time for 5-10 minutes.
[0105] The metal mesh after the corrosion treatment is cleaned to clean the corrosion solution remaining in the metal mesh.
[0106] Preferably, step (d) comprises placing the metal mesh in a crystal planting solution and ultrasonicating for 20-60 minutes, then taking it out and drying it, and the preferred drying method is to blow it dry with nitrogen; the crystal planting solution is preferably a nano-diamond suspension; the nano-diamond suspension preferably comprises nano-diamond powder, dimethyl carbonate and water, the mass of the nano-diamond powder accounts for 0.005-0.01% of the mass of the nano-diamond suspension, and the concentration of dimethyl carbonate in the nano-diamond suspension is 1×10 -6 -10×10 -6 mol / L; preferably the pH of the nanodiamond suspension is 2-4.
[0107] The metal mesh is treated with diamond crystals. The typical crystal solution is a detonation nanodiamond suspension, which has a diamond powder mass fraction of 0.005% and a DMC concentration of 5×10 -6 M, the rest is deionized water, and the pH is 3. The crystal planting method is to put the sample into the crystal planting solution for ultrasonication for 30 minutes, take it out, and blow it dry with nitrogen.
[0108] Step (e) deposits a diamond coating on the surface of the metal mesh by hot wire chemical vapor deposition, which is the same as described above.
[0109] The typical preparation method of the diamond-coated metal mesh increases the growth nucleation density and secondary nucleation rate through a surface pretreatment method of corrosion treatment and crystal planting treatment before hot wire chemical vapor deposition, thereby obtaining a film with a nano-sized grain size. The prepared diamond-coated metal mesh has high oil-water separation efficiency and a long service life.
[0110] According to a second aspect of the present invention, there is provided a metal mesh coating deposition device for hot wire chemical vapor deposition in the above-mentioned method for preparing the oil-water separation diamond coated metal mesh, such as Figure 1 , Figure 2 As shown, the metal mesh coating deposition device includes a clamp body 100 located between the upper and lower heat discharge wires 300; the clamp body 100 includes a first body 110 and a second body 120 arranged in parallel, and the first body 110 and the second body 120 have cavities inside the bodies independently, and the metal mesh 200 is placed between the first body 110 and the second body 120, and the edge size of the metal mesh 200 is larger than the cavity size of the first body 110 and the second body 120, and the first body 110 and the second body 120 are fixed by a detachable clamping mechanism 130 perpendicular to the first body 110 to clamp the metal mesh 200 between the first body 110 and the second body 120.
[0111] When in use, the metal mesh 200 is placed between the first body 110 and the second body 120, and the first body 110 and the second body 120 are clamped by the detachable clamping mechanism 130, so as to clamp the metal mesh 200 therebetween. Since the space between the first body 110 and the second body 120 is empty, the edge size of the metal mesh 200 is larger than the hole size of the first body 110 and the second body 120, and the metal mesh 200 can be mounted between the first body 110 and the second body 120. The shape of the hole is not limited, as long as the edge of the metal mesh 200 is mounted between the first body 110 and the second body 120 and does not jump out, a clamp is formed. When depositing the coating, the device is placed in the deposition substrate position.
[0112] The hot wire chemical vapor deposition device designed in the present invention has a simple structure and can fix the metal mesh. The metal mesh will not be deformed during the deposition process and is very suitable for the preparation of chemical vapor deposition coatings in a three-dimensional direction. At the same time, by using the device, the deposition temperature of the metal mesh is made more uniform. When the designed device is used to deposit a low-temperature nano-diamond coating, the diamond film grows uniformly, and the obtained diamond-coated metal mesh has a better oil-water separation effect.
[0113] Preferably, the first body and the second body are both molybdenum disks.
[0114] Molybdenum has a high melting point and can maintain high strength at high temperatures. It also has a high elastic modulus and low weight, making it an ideal carrier material for the fixture body.
[0115] Preferably, the detachable clamping mechanism 130 includes a bolt 131 and a nut 132 .
[0116] The detachable clamping mechanism includes multiple sets of bolts and nuts. Multiple bolts pass through the parallel first body and second body, and the nuts are used to adjust the distance between the first body and the second body. They are tightened to clamp the metal mesh in the middle, fix the metal mesh, and prevent the metal mesh from deforming under high temperature.
[0117] In a preferred embodiment, the clamp body 100 further includes a first spring piece 141 and / or a second spring piece 142 ; the first spring piece 141 is located inside the first body 110 ; and the second spring piece 142 is located inside the second body 120 .
[0118] The inner side here refers to the side where the metal mesh contacts the body.
[0119] By providing the first spring sheet and / or the second spring sheet, gaps can be avoided when the metal mesh is fixed with bolts and nuts, so that the metal mesh is clamped and fixed more firmly, and deformation of the metal mesh is further prevented.
[0120] According to a third aspect of the present invention, there is provided a diamond coated metal mesh prepared by the above-mentioned method for preparing the oil-water separation diamond coated metal mesh, or a diamond coated metal mesh obtained by hot wire chemical vapor deposition using the above-mentioned metal mesh coating deposition device.
[0121] The diamond-coated metal mesh prepared by the method or the diamond-coated metal mesh obtained by hot-wire chemical vapor deposition using the device has good oil-water separation effect, high oil-water separation efficiency and long service life of the metal mesh.
[0122] According to a fourth aspect of the present invention, there is provided a use of the diamond-coated metal mesh in oil-water separation.
[0123] Since the obtained diamond-coated metal mesh has hydrophobicity and oleophilicity, it can be used in oil-water separation, has good separation effect, high efficiency, long service life, and has broad application prospects.
[0124] Preferably, it can be used for the separation of oily wastewater including common organic solvents, animal and vegetable oils, petroleum, gasoline, diesel and crude oil.
[0125] Preferably, the diamond-coated metal mesh is placed in an oil-water mixture, and the oil can pass through the diamond-coated metal mesh but the water cannot pass through the diamond-coated metal mesh, thereby achieving the purpose of oil-water separation.
[0126] When separating oil and water, the metal mesh can be made into various shapes according to the actual situation. For example, the oil-water mixture is poured on the metal mesh, and the oil drips (filters) through the metal mesh, while the water remains on the surface of the metal mesh. For another example, the metal mesh can be surrounded by a fence (surrounded by a circle) and placed in the oil-water mixture. The oil enters the fence surrounded by the metal mesh and is collected (collected), while the water does not enter the metal mesh. This method can be used to treat marine oil pollution.
[0127] According to a fifth aspect of the present invention, there is provided an oil-water separation device comprising the above-mentioned diamond-coated metal mesh.
[0128] The oil-water separator has the same advantages as the diamond-coated metal mesh described above.
[0129] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. All raw materials involved in the present invention can be obtained through commercial purchase.
[0130] The metal mesh in the examples and comparative examples is a copper mesh.
[0131] The detonation nano-diamond suspension used in the embodiment and the comparative example has a diamond powder mass fraction of 0.005%, a DMC concentration of 5×10 -6 M, the rest is deionized water, pH is 3.
[0132] Example 1
[0133] A method for preparing a diamond-coated metal mesh comprises the following steps:
[0134] (1) Clean the surface of the metal mesh by ultrasonically cleaning it twice with deionized water for 5 minutes each time, and finally ultrasonically cleaning it with alcohol for 5 minutes, and then blowing it dry with nitrogen;
[0135] (2) The cleaned metal mesh is subjected to corrosion treatment to increase the surface roughness and improve the adsorption density of diamond nanoparticles. The corrosion treatment is ultrasonic cleaning in an alkaline solution for 5 minutes and then cleaning in an acid solution for 30 seconds. The alkaline solution is 1M NaOH and the acid solution is 1M HCl;
[0136] (3) Clean the metal mesh to remove the corrosion solution remaining in the metal mesh. Use deionized water to ultrasonically clean it twice, 5 minutes each time, and finally use alcohol to ultrasonically clean it for 5 minutes, and blow it dry with nitrogen;
[0137] (4) The metal mesh is treated with nano-diamond crystals. The crystal planting solution is a detonation nano-diamond suspension. The crystal planting method is to put the sample into the crystal planting solution and ultrasonicate it for 30 minutes, then take it out and blow it dry with nitrogen;
[0138] (5) Use hot wire CVD to prepare three-dimensional nanodiamond film on the metal mesh after crystal planting, and heat it from room temperature to 600℃ at a rate of 20℃ / min, and keep it warm for 15 minutes; during the reaction, the total gas flow rate is controlled to be 500mL / min, and the total flow rate of methane + argon + hydrogen is 500mL / min, including 10mL / min of methane, 282mL / min of argon, and 208mL / min of hydrogen. The pressure is 1500Pa. The distance between the upper row of hot wires and the sample is 25mm, and the distance between the lower row of hot wires and the sample is 15mm. The deposition time is 2 hours.
[0139] Figure 3 This is the surface morphology of the metal mesh in Example 1; Figure 4 This is the surface morphology of the diamond film grown on the metal mesh in Example 1.
[0140] Example 2
[0141] A method for preparing a diamond-coated metal mesh comprises the following steps:
[0142] (1) Clean the surface of the metal mesh by first using deionized water for ultrasonic cleaning three times, each time for 5 minutes, and finally using alcohol for ultrasonic cleaning for 5 minutes, and then blowing dry with nitrogen.
[0143] (2) The cleaned metal mesh is subjected to corrosion treatment to increase the surface roughness and improve the adsorption density of diamond nanoparticles. The corrosion treatment is ultrasonic cleaning in an alkaline solution for 10 minutes and then cleaning in an acid solution for 60 seconds. The alkaline solution is 0.5M NaOH and the acid solution is 0.5M HCl.
[0144] (3) Clean the metal mesh to remove the corrosion solution remaining in the metal mesh. Use deionized water for ultrasonic cleaning three times, 5 minutes each time, and finally use alcohol for ultrasonic cleaning for 5 minutes, and blow dry with nitrogen.
[0145] (4) The metal mesh is treated with nano-diamond crystals, and the crystal-planting solution is a detonation nano-diamond suspension. The crystal-planting method is to put the sample into the crystal-planting solution for ultrasonication for 30 minutes, take it out, and blow it dry with nitrogen.
[0146] (5) Use hot wire CVD to prepare three-dimensional nanodiamond film on the metal mesh after crystal planting, and heat it from room temperature to 600℃ at a heating rate of 20℃ / min, and keep it warm for 15 minutes; during the reaction, the total gas flow rate is controlled to be 400mL / min, and the total flow rate of methane + argon + hydrogen is 400mL / min, including 5mL / min of methane, 255mL / min of argon, and 140mL / min of hydrogen. The pressure is 1500Pa. The distance between the upper row of hot wires and the sample is 25mm, and the distance between the lower row of hot wires and the sample is 15mm. The deposition time is 3 hours.
[0147] Example 3
[0148] A method for preparing a diamond-coated metal mesh comprises the following steps:
[0149] (1) Clean the surface of the metal mesh by first using deionized water for ultrasonic cleaning twice, each time for 10 minutes, and finally using alcohol for ultrasonic cleaning for 5 minutes, and then blowing dry with nitrogen.
[0150] (2) The cleaned metal mesh is subjected to corrosion treatment to increase the surface roughness and improve the adsorption density of diamond nanoparticles. The corrosion treatment is ultrasonic cleaning in an alkaline solution for 8 minutes and then cleaning in an acid solution for 40 seconds. The alkaline solution is 0.6M NaOH and the acid solution is 0.6M HCl.
[0151] (3) Clean the metal mesh to remove the corrosion solution remaining in the metal mesh. Use deionized water for ultrasonic cleaning twice, 10 minutes each time, and finally use alcohol for ultrasonic cleaning for 5 minutes, and blow dry with nitrogen.
[0152] (4) The metal mesh is treated with nano-diamond crystals, and the crystal-planting solution is a detonation nano-diamond suspension. The crystal-planting method is to put the sample into the crystal-planting solution for ultrasonication for 30 minutes, take it out, and blow it dry with nitrogen.
[0153] (5) Use hot wire CVD to prepare three-dimensional nanodiamond film on the metal mesh after crystal planting, and heat up from room temperature to 600℃ at a rate of 20℃ / min, and keep warm for 15 minutes; during the reaction, the total gas flow rate is controlled to be 420mL / min, and the total flow rate of methane + argon + hydrogen is 420mL / min, including 15mL / min of methane, 255mL / min of argon, and 150mL / min of hydrogen. The pressure is 1500Pa. The distance between the upper row of hot wires and the sample is 25mm, and the distance between the lower row of hot wires and the sample is 15mm. The deposition time is 1.5 hours.
[0154] Example 4
[0155] A method for preparing a diamond-coated metal mesh comprises the following steps:
[0156] (1) Clean the surface of the metal mesh by first using deionized water for ultrasonic cleaning twice, each time for 5 minutes, and finally using alcohol for ultrasonic cleaning for 10 minutes, and then blowing dry with nitrogen.
[0157] (2) The cleaned metal mesh is subjected to corrosion treatment to increase the surface roughness and improve the adsorption density of diamond nanoparticles. The corrosion treatment is ultrasonic cleaning in an alkaline solution for 5 minutes and then cleaning in an acid solution for 30 seconds. The alkaline solution is 1M NaOH and the acid solution is 1M HCl.
[0158] (3) Clean the metal mesh to remove the corrosion solution remaining in the metal mesh. Use deionized water for ultrasonic cleaning twice, 5 minutes each time, and finally use alcohol for ultrasonic cleaning for 10 minutes, and blow dry with nitrogen.
[0159] (4) The metal mesh is treated with nano-diamond crystals, and the crystal-planting solution is a detonation nano-diamond suspension. The crystal-planting method is to put the sample into the crystal-planting solution for ultrasonication for 20 minutes, take it out, and blow it dry with nitrogen.
[0160] (5) Use hot wire CVD to prepare three-dimensional nanodiamond film on the metal mesh after crystal planting, and heat up from room temperature to 500°C at a rate of 15°C / min, and keep warm for 20 minutes; during the reaction, the total gas flow rate is controlled to be 500mL / min, and the total flow rate of methane + argon + hydrogen is 500mL / min, including 5mL / min of methane, 255mL / min of argon, and 140mL / min of hydrogen. The pressure is 2000Pa. The distance between the upper row of hot wires and the sample is 25mm, and the distance between the lower row of hot wires and the sample is 15mm. The deposition time is 4 hours.
[0161] Example 5
[0162] A method for preparing a diamond-coated metal mesh comprises the following steps:
[0163] (1) Clean the surface of the metal mesh by first using deionized water for ultrasonic cleaning twice, each time for 5 minutes, and finally using alcohol for ultrasonic cleaning for 5 minutes, and then blowing dry with nitrogen.
[0164] (2) The cleaned metal mesh is subjected to corrosion treatment to increase the surface roughness and improve the adsorption density of diamond nanoparticles. The corrosion treatment is ultrasonic cleaning in an alkaline solution for 5 minutes and then cleaning in an acid solution for 30 seconds. The alkaline solution is 1M NaOH and the acid solution is 1M HCl.
[0165] (3) Clean the metal mesh to remove the corrosion solution remaining in the metal mesh. Use deionized water for ultrasonic cleaning twice, 5 minutes each time, and finally use alcohol for ultrasonic cleaning for 5 minutes, and blow dry with nitrogen.
[0166] (4) The metal mesh is treated with nano-diamond crystals, and the crystal-planting solution is a detonation nano-diamond suspension. The crystal-planting method is to put the sample into the crystal-planting solution for ultrasonic treatment for 60 minutes, take it out, and blow it dry with nitrogen.
[0167] (5) Use hot wire CVD to prepare three-dimensional nanodiamond film on the metal mesh after crystal planting, and heat it from room temperature to 800℃ at a rate of 25℃ / min, and keep it warm for 10 minutes; during the reaction, the total gas flow rate is controlled to be 500mL / min, and the total flow rate of methane + argon + hydrogen is 500mL / min, including 5mL / min of methane, 255mL / min of argon, and 140mL / min of hydrogen. The pressure is 1500Pa. The distance between the upper row of hot wires and the sample is 20mm, and the distance between the lower row of hot wires and the sample is 18mm. The deposition time is 2 hours.
[0168] Example 6
[0169] A method for preparing a diamond-coated metal mesh, which is different from Example 1 in that in step (5), the temperature is raised from room temperature to 1000° C. at a heating rate of 20° C. / min and maintained for 15 minutes.
[0170] Example 7
[0171] A method for preparing a diamond-coated metal mesh, which is different from Example 1 in that the total gas flow rate in step (5) is controlled to be 500 mL / min, and the total flow rate of methane + argon + hydrogen is 500 mL / min, including 50 mL / min of methane, 282 mL / min of argon, and 168 mL / min of hydrogen.
[0172] Example 8
[0173] A method for preparing a diamond-coated metal mesh, which is different from Example 1 in that step (5) uses a metal mesh coating deposition device to prepare a three-dimensional nano-diamond film on the metal mesh after crystal planting.
[0174] The metal mesh coating deposition device includes a fixture body located between upper and lower heat dissipation wires; the fixture body includes upper and lower molybdenum disks arranged in parallel, and spring sheets are provided on the inner sides of the upper and lower molybdenum disks. The metal mesh is placed between the spring sheets of the molybdenum disks. Bolts are vertically inserted into the fixture body and pass through the upper and lower molybdenum disks, and tightened with nuts to clamp the metal mesh.
[0175] Comparative Example 1
[0176] A method for preparing a diamond-coated metal mesh, which is different from Example 2 in that step (5) uses a microwave plasma CVD method to prepare a three-dimensional nanodiamond film on the metal mesh after crystal planting. The experimental conditions are: the total flow rate of the reaction gas is 300 sccm, the ratio is H 2 :CH 4=292:8 (sccm), pressure is 130 Torr, microwave power is 1.7 kW, deposition substrate temperature is about 800°C, deposition time is 7 h, and the obtained diamond film thickness is about 2 μm.
[0177] Comparative Example 2
[0178] A method for preparing a diamond-coated metal mesh, which is different from Example 2 in that step (5) uses a flame combustion method to prepare a three-dimensional nanodiamond film on the metal mesh after crystal planting. The experimental conditions are: the total flow rate of the reaction gas is 500 sccm, the ratio is H 2 :C 2 H 2 :O 2 =5:245:250 (sccm), the pressure is 1000Pa, the deposition substrate temperature is about 1000℃, the deposition time is 5h, and the diamond film thickness is about 2μm.
[0179] Test example
[0180] The diamond-coated metal mesh obtained in Example 1 was measured using a contact angle meter. The contact angle of the surface of the diamond-coated metal mesh to 3 microliters of n-hexane in an air environment was less than 15°, indicating that it was a superhydrophobic material. The diamond-coated metal mesh was then immersed in n-hexane, and the contact angle of the surface of the metal mesh to 3 microliters of water was measured to be greater than 135°, indicating that it was an oleophilic material.
[0181] In order to examine the oil-water separation performance of the diamond-coated metal mesh obtained in the examples and comparative examples, the oil-water separation efficiency and service life were tested as follows:
[0182] (1) Oil-water separation efficiency: The obtained metal mesh is placed in the middle of a vertically placed filter and fixed with a clip. n-hexane and water are added in a ratio of 1:2 under magnetic stirring to obtain an oil-water mixture, which is poured into the filter through the inlet of the upper part. The n-hexane in the mixture quickly passes through the metal mesh, while the water is blocked above the metal mesh and cannot pass through, thus achieving oil-water separation. The separation efficiency is obtained by calculating the ratio of the weight of water retained above the metal mesh to the weight of water originally poured into the oil-water mixture.
[0183] (2) Service life: The obtained metal mesh was repeatedly used according to the above oil-water separation test, and was cleaned with water after each use. The separation efficiency was calculated after 50 uses.
[0184] The test results are shown in Table 1.
[0185] Table 1
[0186]
[0187]
[0188] From the results in Table 1, it can be seen that the metal mesh obtained by the method of the present invention has a high oil-water separation efficiency of more than 99%, and after being reused 50 times, the separation efficiency remains almost unchanged, still as high as more than 98%, which shows that the prepared metal mesh has excellent recyclability and a long service life.
[0189] Further analysis shows that the hot wire CVD reaction temperature in Example 1 is lower than that in Example 6. It is found that the metal mesh obtained in Example 1 has better oil-water separation efficiency and service life. This is because the lower temperature will not cause deformation of the metal mesh, and the obtained diamond film has better quality. Compared with Example 7, the ratio of hydrogen and methane gas in Example 1 is within the preferred range of the present invention. It is found that the metal mesh obtained in Example 1 has better oil-water separation performance. It can be seen that the diamond film quality and performance obtained by using a certain ratio of hydrogen and methane gas is better.
[0190] Example 8 Compared with Example 1, the deposition device designed by the present invention is used to carry out hot wire CVD deposition. It is found that the metal mesh obtained after deposition has better oil-water separation performance. This is because the device can prevent the metal mesh from deforming and make the deposition temperature of the metal mesh more uniform, making the growth of the diamond film more uniform. The obtained metal mesh has better hydrophobic and oleophilic properties and higher separation efficiency.
[0191] Comparative Example 1 uses a microwave plasma CVD method to deposit a diamond coating. Although it also has a good oil-water separation effect, the deposition equipment is expensive and costly, and diamond films can only be grown on small-sized workpieces. The metal mesh for oil-water separation is large in area, so this method of depositing diamond films on the surface of the metal mesh is only suitable for laboratory research, and is not suitable for industrial production and a large number of industrial uses.
[0192] Comparative Example 2 uses flame combustion method to deposit diamond coating, and the oil-water separation performance of the obtained metal mesh is worse than that of the present invention.
[0193] In summary, the present invention grows nanodiamonds through hot wire chemical vapor deposition and a metal mesh deposition coating device, which effectively avoids deformation of the metal mesh during the deposition process. This method has a fast film formation rate, a simple preparation process, a stable process, and a low cost. It is suitable for industrial production and large-scale industrial use. The resulting metal mesh has high oil-water separation efficiency and a long service life.
[0194] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications that fall within the scope of the present invention in the appended claims.
Claims
1. A method for preparing a diamond-coated metal mesh for oil-water separation, characterized in that: The following steps are involved: (a) Cleaning the surface of the metal mesh; (b) performing corrosion treatment on the cleaned metal mesh; (c) re-cleaning the metal mesh; (d) performing nano-diamond crystal planting on the metal mesh; (e) after the crystal planting treatment, a diamond coating is deposited on the surface of the metal mesh by hot wire chemical vapor deposition to obtain a diamond coated metal mesh; During hot-wire chemical vapor deposition, the gas sources include hydrogen and methane gases, and the temperature of the reaction zone is 600°C; The temperature of the reaction zone was raised from room temperature to 600 °C at a heating rate of 20 °C / min and kept at this temperature for 15 min; The gas source also includes inert gas; during the reaction, the total flow rate of hydrogen, methane and inert gas is 500 mL / min, including 10 mL / min of methane, 282 mL / min of argon and 208 mL / min of hydrogen; The deposition pressure is 1500Pa; The vertical distance between the upper row of hot wires and the metal mesh is 25 mm, and the vertical distance between the lower row of hot wires and the metal mesh is 15 mm; The deposition time was 2 h; Step (b) comprises first ultrasonicating in an alkaline solution for 5 minutes and then ultrasonicating in an acid solution for 30 seconds; the alkaline solution is a 1 mol / L NaOH solution; the acid solution is a 1 mol / L HCl solution; The crystal planting treatment includes placing the metal mesh in the crystal planting solution and ultrasonicating for 30 minutes, then taking it out and drying it, and the drying method is to blow it dry with nitrogen; The planting solution is a nano-diamond suspension; the nano-diamond suspension includes nano-diamond powder, dimethyl carbonate and water, the mass of the nano-diamond powder accounts for 0.005% of the mass of the nano-diamond suspension, and the concentration of dimethyl carbonate in the nano-diamond suspension is 5×10 -6 mol / L; the pH of the nanodiamond suspension is 3; A diamond-coated metal mesh obtained by hot-wire chemical vapor deposition using a metal mesh coating deposition device; The metal mesh coating deposition device comprises a clamp body (100) located between upper and lower heat exhaust wires (300); The clamp body (100) comprises a first body (110) and a second body (120) arranged in parallel, the first body (110) and the second body (120) each independently have a cavity inside the body, a metal mesh (200) is placed between the first body (110) and the second body (120), and the edge size of the metal mesh (200) is larger than the cavity size of the first body (110) and the second body (120), and the first body (110) and the second body (120) are fixed by a detachable clamping mechanism (130) perpendicular to the first body (110) to clamp the metal mesh (200) between the first body (110) and the second body (120); The clamp body (100) further comprises a first spring sheet (141) and a second spring sheet (142); The first spring sheet (141) is located inside the first body (110); The second spring sheet (142) is located inside the second body (120).
2. The method for preparing the diamond-coated metal mesh for oil-water separation according to claim 1, characterized in that: Step (a) and step (c) independently include first ultrasonic cleaning with water for 2-3 times, each time for 5-10 minutes, and then ultrasonic cleaning with alcohol for 1-2 times, each time for 5-10 minutes.
3. According to the method for preparing the oil-water separation diamond-coated metal mesh as claimed in claim 1, the metal mesh is a copper mesh, a titanium mesh or a stainless steel mesh.
4. The method for preparing the diamond-coated metal mesh for oil-water separation according to any one of claims 1 to 3, characterized in that: The first body (110) and the second body (120) are both molybdenum disks; The detachable clamping mechanism (130) comprises a bolt (131) and a nut (132).