Curable resin composition, dry film, cured product and printed circuit board
By introducing polyester with aromatic structure and polyether structure into the curable resin composition, the problems of chemical tin plating resistance and soldering heat resistance are solved, and a high-resolution and non-sticky cured coating is achieved.
Patent Information
- Application Number
- CN201910244783.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-03-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-03-28
AI Technical Summary
When improving the resistance to electroless tin plating, existing curable resin compositions lead to deterioration in touch dryness, poor soldering heat resistance and other characteristics, and are difficult to maintain excellent developability and resolution.
A dry film is formed by photocuring and thermal curing using a curable resin composition containing a carboxyl-containing resin, a photopolymerization initiator, a thermosetting compound, a photopolymerizable monomer, and a polyester having both an aromatic structure and a polyether structure. , adjust solubility and softness to improve chemical tin plating resistance and soldering heat resistance.
While maintaining resolution and non-stick properties, the chemical tin plating resistance and soldering heat resistance are significantly improved, forming a cured coating with excellent characteristics.
Smart Images

Figure BDA0002010754760000211
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin composition, a dry film and a cured product thereof suitable for forming a coating such as a solder mask layer of a printed circuit board, and more specifically, to a curable resin composition, a dry film and a cured product thereof capable of forming a pattern of a cured coating having excellent dryness to touch (non-stickiness), resolution, chemical tin plating resistance and soldering heat resistance of the dry coating. The present invention also relates to a printed circuit board formed by forming a permanent coating such as a solder mask layer from the cured product of the above composition. Background Art
[0002] In the past, curable resin compositions that can be developed with an alkaline aqueous solution have been widely used as materials for forming permanent coating patterns such as solder resist layers in printed circuit boards by exposure and development. For example, a curable resin composition is listed, which includes: a carboxyl-containing resin obtained by adding a polyacid anhydride to a reaction product of a novolac epoxy resin and an unsaturated monocarboxylic acid; a photopolymerization initiator; a diluent; and an epoxy resin (see Patent Document 1).
[0003] According to such a curable resin composition, the developability and resolution are excellent, and after the pattern is formed, it is thermally cured, so that a three-dimensional network structure is formed by the addition reaction of the carboxyl group remaining in the coating film and the epoxy group, and a cured film with excellent adhesion, hardness, heat resistance, chemical gold plating resistance, electrical insulation, etc. can be obtained.
[0004] On the other hand, in the manufacturing process of a printed wiring board, after forming a cured film such as a solder resist layer, generally, plating is applied to connection terminals such as conductor pads as a pre-treatment for surface protection of the conductor or for bonding.
[0005] As such plating, chemical gold plating has been used because it does not require electricity or lead plating. However, recently, chemical tin plating has been used in comparison with chemical gold plating in terms of cost, chemical safety, and the like.
[0006] This chemical tin plating is an immersion plating method, which dissolves the copper surface as a conductor layer while precipitating tin. Therefore, there is a problem that the chemical solution of the chemical tin plating invades the interface between the solder resist layer and the copper in the pattern opening of a permanent coating such as a solder resist layer formed by the curable resin composition described in Patent Document 1, causing the solder resist layer to peel off.
[0007] In view of this, it is required to develop a curable resin composition with excellent resistance to chemical tin plating, but it is noted that if the resistance to chemical tin plating is to be improved, the following new problems will arise: the dryness to touch (non-stickiness) of the dried coating surface will deteriorate, and when a negative film is brought into contact and exposed, contact marks of the negative film will be generated on the dried coating surface.
[0008] Patent Document 1: Japanese Patent Publication No. 1-54390 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] Therefore, an object of the present invention is to provide a curable resin composition capable of forming a pattern of a cured film, which maintains original characteristics such as excellent developability and resolution, has excellent resistance to chemical tin plating after curing without causing problems such as deterioration of dryness to touch (non-tackiness), and also has excellent characteristics such as adhesion to various substrates, resistance to soldering heat, moisture resistance, chemical resistance, and electrical insulation.
[0011] Solutions for solving problems
[0012] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that polyester having both an aromatic structure and a polyether structure can improve adhesion to copper as a substrate without reducing the developability and heat resistance of the curable resin composition, thereby completing the present invention.
[0013] That is, the curable resin composition of the present invention is characterized by comprising: (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) a thermosetting compound, (D) a photopolymerizable monomer, and (E) a polyester having both an aromatic structure and a polyether structure.
[0014] In the curable resin composition of the present invention, the polyester (E) having both an aromatic structure and a polyether structure is preferably a polyester obtained by reacting an alkylene oxide adduct of bisphenol with a polycarboxylic acid.
[0015] It is believed that the thermal stability is improved by utilizing the aromatic structure of bisphenol or the like, the flexibility is imparted by utilizing the introduced polyether structure by being an alkylene oxide adduct, and the solubility as a composition can be adjusted to be optimal by utilizing the polyester obtained by reacting with a polycarboxylic acid, thereby improving the soldering heat resistance and chemical tin plating resistance.
[0016] The dry film of the present invention is characterized in that it is obtained by applying the curable resin composition on a thin film and drying it.
[0017] The cured product of the present invention is characterized in that it is obtained by subjecting the aforementioned curable resin composition or the curable resin composition constituting the aforementioned dry film to at least one of photocuring and thermal curing.
[0018] The printed wiring board of the present invention is characterized by comprising the above-mentioned cured product.
[0019] Effects of the Invention
[0020] According to the present invention, it is possible to provide a curable resin composition which maintains resolution and the non-tackiness of a dried coating film and has improved resistance to chemical tin plating and resistance to soldering heat compared to the prior art. DETAILED DESCRIPTION
[0021] Hereinafter, the curable resin composition of the present invention will be specifically described, but the present invention is not limited thereto at all.
[0022] In addition, when the described compound exists in isomers, all the isomers that can exist can be used in the present invention unless otherwise specified.
[0023] <Composition of curable resin composition>
[0024] The curable resin composition of the present invention has the following characteristics: it comprises (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) a thermosetting compound, (D) a photopolymerizable monomer, and (E) a polyester having both an aromatic structure and a polyether structure. It should be noted that the curable resin composition of the present invention may contain other optional components such as an inorganic filler within the range that does not hinder the effect of the present invention.
[0025] [(A) Carboxyl group-containing resin]
[0026] As the carboxyl group-containing resin, any known resin may be used as long as it has a carboxyl group in its molecule. The carboxyl group-containing resin may be used alone or in combination of two or more.
[0027] As the carboxyl group-containing resin, from the aspects of photocurability and development resistance, a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is preferred. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. By using a carboxyl group-containing resin having an ethylenically unsaturated double bond, the composition is easily photocurable.
[0028] Specific examples of the carboxyl group-containing resin include the following compounds (both oligomers and polymers).
[0029] (I) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, a lower alkyl (meth)acrylate, or isobutylene.
[0030] (II) A carboxyl-containing polyurethane resin obtained by a polyaddition reaction of a diisocyanate such as an aliphatic diisocyanate, a branched aliphatic diisocyanate, an alicyclic diisocyanate, an aromatic diisocyanate, a carboxyl-containing diol compound such as dimethylol propionic acid and dimethylol butyric acid, and a diol compound such as a polycarbonate polyol, a polyether polyol, a polyester polyol, a polyolefin polyol, an acrylic polyol, a bisphenol A-based alkylene oxide adduct diol, and a compound having a phenolic hydroxyl group and an alcoholic hydroxyl group.
[0031] (III) A carboxyl-containing photosensitive polyurethane resin obtained by a polyaddition reaction of a diisocyanate, a (meth)acrylate of a bifunctional epoxy resin such as a bisphenol A epoxy resin, a hydrogenated bisphenol A epoxy resin, a bisphenol F epoxy resin, a bisphenol S epoxy resin, a bixylenol epoxy resin, a biphenol epoxy resin or a partially anhydride-modified product thereof, a carboxyl-containing diol compound and a diol compound.
[0032] (IV) A carboxyl-containing photosensitive polyurethane resin is prepared by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as hydroxyalkyl (meth)acrylate to the synthesis of the resin of (II) or (III) above to obtain a terminally (meth)acryloyl-containing photosensitive polyurethane resin.
[0033] (V) In the synthesis of the resin of the above (II) or (III), a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reaction product of isophorone diisocyanate and pentaerythritol triacrylate, is added to obtain a carboxyl-containing photosensitive polyurethane resin whose terminals are (meth)acryloylated.
[0034] (VI) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or higher-functional (solid) epoxy resin with (meth)acrylic acid to add a dibasic acid anhydride to a hydroxyl group present in a side chain.
[0035] (VII) A carboxyl group-containing photosensitive resin obtained by further epoxidizing the hydroxyl groups of a bifunctional (solid) epoxy resin with epichlorohydrin to obtain a polyfunctional epoxy resin, reacting the obtained polyfunctional epoxy resin with (meth)acrylic acid, and adding a dibasic acid anhydride to the generated hydroxyl groups.
[0036] (VIII) A carboxyl group-containing polyester resin obtained by reacting a bifunctional oxetane resin with a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid, and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the generated primary hydroxyl group.
[0037] (IX) A carboxyl-containing resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule such as p-hydroxyphenylethanol and a monocarboxylic acid containing an unsaturated group such as (meth)acrylic acid to obtain a reaction product, and reacting the alcoholic hydroxyl group of the obtained reaction product with a polyacid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, etc.
[0038] (X) A carboxyl-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the reaction product obtained with a polyacid anhydride.
[0039] (XI) A carboxyl-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate to obtain a reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the reaction product with a polyacid anhydride.
[0040] (XII) A carboxyl-containing photosensitive resin obtained by adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins of (I) to (XI).
[0041] The acid value of the carboxyl-containing resin is preferably in the range of 30 to 150 mgKOH / g, more preferably in the range of 50 to 120 mgKOH / g. By setting the acid value of the carboxyl-containing resin to 30 mgKOH / g or more, alkali development becomes easy. In addition, by setting it to 150 mgKOH / g or less, dissolution of the exposed portion caused by the developer is prevented, and the unexposed portion is dissolved and peeled off, making it easy to draw a normal resist pattern.
[0042] The weight average molecular weight (hereinafter, sometimes abbreviated as Mw) of the carboxyl-containing resin varies depending on the resin skeleton. Generally speaking, it is preferably in the range of 2000 to 150000, and further in the range of 3000 to 100000. If the weight average molecular weight is 2000 or more, the moisture resistance of the resin layer after exposure is good, film loss is not easy to occur during development, and the resolution becomes good. In addition, if the weight average molecular weight is 150000 or less, the development resistance and storage stability become good. The weight average molecular weight can be measured by gel permeation chromatography.
[0043] The carboxyl resin can be used without being limited to the above-mentioned enumeration. Among them, the carboxyl resin synthesized using phenolic compounds as starting materials has excellent HAST resistance (super accelerated life test) and PCT resistance (saturated vapor pressure test), so it can be preferably used.
[0044] The amount of the carboxyl-containing resin is preferably 5 to 60% by mass, more preferably 10 to 60% by mass, further preferably 15 to 60% by mass, and particularly preferably 20 to 50% by mass, based on the total amount of the resin composition. If it is within this range, the coating strength is good, the viscosity of the composition is appropriate, and the coating properties can be improved.
[0045] [(B) Photopolymerization initiator]
[0046] As the photopolymerization initiator, a known one can be used. In addition, the photopolymerization initiator may be used alone or in combination of two or more.
[0047] Examples of the photopolymerization initiator include diacylphosphine oxides such as bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and 2,6-dimethoxybenzoyldiphenylphosphine oxide. Phosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, methyl 2,4,6-trimethylbenzoylphenylphosphine oxide, 2-methylbenzoyldiphenylphosphine oxide, isopropyl pivaloylphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide and other monoacylphosphine oxides; ethyl phenyl (2,4,6-trimethylbenzoyl) phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one, 2-hydroxy-2-methyl-1-phenylpropane-1-one and other hydroxyacetophenones Benzoin, benzyl and other benzoin; benzoin alkyl ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether and benzoin n-butyl ether; benzophenones such as benzophenone, p-methyl benzophenone, Michler's ketone, methyl benzophenone, 4,4'-dichlorobenzophenone and 4,4'-bis(diethylamino)benzophenone; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone, 2-(dimethylamino)- Acetophenones such as 2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone and N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone; anthraquinones such as anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoates such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate and ethyl p-dimethylbenzoate;Oxime esters such as {1-[4-(phenylthio)-2-(O-benzoyl oxime)]}1,2-octanedione, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-1-(O-acetooxime)ethanone; titanocenes such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium; phenyl disulfide 2-nitrofluorene, butyroquinone, anisole ether, azobisisobutyronitrile, tetramethylthiuram disulfide, etc. ;
[0048] The content of the photopolymerization initiator is preferably 0.1 to 30 parts by mass relative to 100 parts by mass of the carboxyl-containing resin in terms of non-volatile components. When the content is 0.1 parts by mass or more, the photocurability of the resin composition becomes good, the film is not easy to peel, and the film properties such as chemical resistance also become good. In addition, when the content is 30 parts by mass or less, the effect of reducing degassing can be obtained, and the light transmittance of the film becomes good, and the deep curing property is not easy to reduce. More preferably, the content is 0.5 to 20 parts by mass.
[0049] [(C) Thermosetting compound]
[0050] As the thermosetting compound, a known one can be used. In addition, the thermosetting compound can be used alone or in combination of two or more.
[0051] Examples of the thermosetting compound include melamine resins, benzoguanamine resins, amino resins such as melamine derivatives and benzoguanamine derivatives, isocyanate compounds, blocked isocyanate compounds, cyclocarbonate compounds, epoxy compounds, oxetane compounds, episulfide resins, bismaleimide, and carbodiimide resins.
[0052] Examples of the epoxy compound include epoxidized vegetable oils; bisphenol A epoxy resins; hydroquinone epoxy resins; bisphenol epoxy resins; thioether epoxy resins; brominated epoxy resins; phenol novolac epoxy resins; cresol novolac epoxy resins; biphenol novolac epoxy resins; bisphenol F epoxy resins; hydrogenated bisphenol A epoxy resins; glycidylamine epoxy resins; hydantoin epoxy resins; alicyclic epoxy resins; trishydroxyphenylmethane epoxy resins; dixylenol or diphenol epoxy resins or their derivatives. mixture; bisphenol S type epoxy resin; bisphenol A novolac type epoxy resin; tetrahydroxyphenylethane type epoxy resin; heterocyclic epoxy resin; diglycidyl phthalate resin; tetraglycidyl ditoluoyl ethane resin; naphthyl-containing epoxy resin; epoxy resin having a dicyclopentadiene skeleton; glycidyl methacrylate copolymer epoxy resin; copolymerized epoxy resin of cyclohexylmaleimide and glycidyl methacrylate; epoxy-modified polybutadiene rubber derivative; CTBN-modified epoxy resin, etc., but not limited to these. These epoxy resins can be used alone or in combination of two or more.
[0053] Examples of the oxetane compound include bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, (3-ethyl-3-oxetanyl)methyl acrylate, In addition to polyfunctional oxetanes such as (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and oligomers or copolymers thereof, etherified products of oxetane alcohol and resins having hydroxyl groups such as novolac resin, poly(p-hydroxystyrene), Cardo-type bisphenols, calixarene, resorcinol calixarene, or silsesquioxane can also be mentioned. In addition, copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates can also be mentioned.
[0054] Examples of the episulfide resin include bisphenol A type episulfide resins, etc. In addition, an episulfide resin obtained by replacing the oxygen atom of the epoxy group of a novolac type epoxy resin with a sulfur atom using the same synthesis method can also be used.
[0055] Examples of the amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.
[0056] As the isocyanate compound, a polyisocyanate compound may be mixed. As the polyisocyanate compound, aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, naphthalene-1,5-diisocyanate, o-xylene diisocyanate, m-xylene diisocyanate and 2,4-toluene diisocyanate dimer; aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate) and isophorone diisocyanate; alicyclic polyisocyanates such as dicycloheptane triisocyanate; and adducts, uret bodies and isocyanurate bodies of the isocyanate compounds listed above.
[0057] As the blocked isocyanate compound, an addition reaction product of an isocyanate compound and an isocyanate blocking agent can be used. As the isocyanate compound that can react with the isocyanate blocking agent, for example, the above-mentioned polyisocyanate compounds can be cited. As the isocyanate blocking agent, for example, phenol-based blocking agents; lactam-based blocking agents; active methylene-based blocking agents; alcohol-based blocking agents; oxime-based blocking agents; thiol-based blocking agents; amide-based blocking agents; imide-based blocking agents; amine-based blocking agents; imidazole-based blocking agents; imine-based blocking agents, etc. can be cited.
[0058] The content of the thermosetting compound is preferably 0.2 to 2.0 mol, more preferably 0.5 to 1.5 mol, of the number of functional groups of the thermosetting compound that reacts per 1 mol of the carboxyl group contained in the carboxyl group-containing resin.
[0059] [(D) Photopolymerizable monomer]
[0060] Photopolymerizable monomers are compounds having ethylenically unsaturated double bonds, which can be polymerized by addition reaction of ethylenically unsaturated double bonds with each other, for example, by light irradiation. By using photopolymerizable monomers, the resistance of the exposed part to the developer and the solubility of the unexposed part to the developer are increased, thereby improving the resolution.
[0061] Examples of such photopolymerizable monomers include alkyl (meth)acrylates such as 2-ethylhexyl (meth)acrylate and cyclohexyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; mono- or di-(meth)acrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; hexanediol, trimethylolpropane, pentaerythritol, di(trimethylolpropane, and dipentaerythritol); , trihydroxyethyl isocyanurate and other polyols or their ethylene oxide or propylene oxide adducts (meth)acrylates; (meth)acrylates of ethylene oxide or propylene oxide adducts of phenols such as phenoxyethyl (meth)acrylate and polyethoxy di(meth)acrylate of bisphenol A; (meth)acrylates of glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether, triglycidyl isocyanurate; and melamine (meth)acrylate; etc.
[0062] The photopolymerizable monomer can be used alone or in combination of two or more. The content of the photopolymerizable monomer is preferably 5 to 40 parts by mass relative to 100 parts by mass of the carboxyl-containing resin in terms of non-volatile components. When the content of the photopolymerizable monomer is within the above range, the photocurability based on exposure can be improved, and the pattern accuracy can be improved in the development process after exposure. In addition, when the content is less than 40 parts by mass, halos are not easily generated, and good resolution can be obtained.
[0063] [(E) Polyester having both an aromatic structure and a polyether structure]
[0064] The polyester having both an aromatic structure and a polyether structure is a polycondensate of a polycarboxylic acid and a polyol having both an aromatic structure and a polyether structure, and known substances can be used. In addition, the polyester can be used alone or in combination of two or more.
[0065] As the polycarboxylic acid, a known one may be used alone or in combination of two or more. The polycarboxylic acid of the present invention may contain anhydride thereof.
[0066] Examples of the polycarboxylic acid include malonic acid, succinic acid, succinic anhydride, glutaric acid, adipic acid, azelaic acid, sebacic acid, phthalic acid, phthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, isophthalic acid, terephthalic acid, nadic anhydride, maleic acid, maleic anhydride, fumaric acid, itaconic acid, citraconic acid, pimelic acid, suberic acid, dodecanedioic acid, trimellitic acid, trimellitic anhydride, pyromellitic acid and pyromellitic anhydride, and the like can be appropriately selected depending on the solubility of the polyester in the composition.
[0067] As the polyol, any known polyol may be used as long as it includes a polyol having an aromatic structure and a polyether structure. One type may be used alone or two or more types may be used in combination.
[0068] Examples of the polyol having an aromatic structure and a polyether structure include aromatic polyols such as 1,4-benzenedimethanol, 1,3-benzenedimethanol, 1,2-benzenedimethanol, 4,4'-naphthalenedimethanol, and 3,4'-naphthalenedimethanol; 1,2,3-trihydroxybenzene, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 4,4'-dihydroxybenzophenone, dihydroxyacetophenone, 1,1-bis(4-hydroxyphenylene)ethane, bis(4-hydroxyphenyl)methane (also known as bisphenol F), 2,2-bis(4-hydroxyphenyl)propane (also known as bisphenol A), bis(4 -hydroxyphenyl) sulfone (also called bisphenol S), bis(4-hydroxyphenyl) ether, 4,4'-biphenol, 1,1-bis(4-hydroxyphenyl) isobutane, 2,2-bis(4-hydroxy-tert-butylphenyl) propane, 2-methyl-1,1-bis(4-hydroxyphenyl) propane, catechol, resorcinol, hydroquinone, novolac, cresol, 1,1,1-(4-hydroxyphenyl) ethane and other polyphenols; bis-(2-hydroxynaphthyl) methane, 1,5-dihydroxy-naphthalene and other dihydroxynaphthalenes and other naphthalene polyols, and derivatives obtained by adding alkylene oxides thereto.
[0069] Among them, the polyol is preferably a polyol obtained by adding alkylene oxide having flexibility to bisphenols such as 1,1-bis(4-hydroxyphenylene)ethane having excellent thermal stability, and more preferably a polyol obtained by adding alkylene oxide to 2,2-bis(4-hydroxyphenyl)propane ("bisphenol A").
[0070] In order to achieve good balance between chemical tin plating resistance and soldering heat resistance, the polyol is preferably a polyol obtained by adding 2 to 30 moles of alkylene oxide to bisphenols, and more preferably a polyol obtained by adding 4 to 20 moles of alkylene oxide. By adding 2 moles or more of alkylene oxide, flexibility and adhesion to copper as a substrate are excellent, and sufficient chemical tin plating resistance can be obtained. By setting the amount to less than 30 moles, a curable resin composition excellent in soldering heat resistance, dryness to touch, and surface hardness can be obtained.
[0071] Furthermore, the alkylene oxide is preferably ethylene oxide, propylene oxide, or butylene oxide.
[0072] As a method for adding alkylene oxide to bisphenols, for example, there can be mentioned a method in which bisphenols are used as initiators and alkylene oxide is added by a known common method. In addition, a known esterification catalyst can be used during the reaction.
[0073] Examples of the esterification catalyst include organic titanium compounds such as tetrabutyl titanate, tetrapropyl titanate, and tetraethyl titanate, and tin compounds such as tin octylate, dibutyltin oxide, dibutyltin laurate, stannous chloride, and stannous bromide.
[0074] The content of the polyester having both an aromatic structure and a polyether structure is preferably 1 to 50 parts by mass relative to 100 parts by mass of the carboxyl group-containing resin in terms of non-volatile components. When the content of the polyester having both an aromatic structure and a polyether structure is within the above range, a curable resin composition having excellent chemical tin plating resistance and soldering heat resistance can be obtained without deteriorating resolution.
[0075] The number average molecular weight (hereinafter sometimes referred to as Mn) of the polyester having both an aromatic structure and a polyether structure is preferably in the range of 3000 to 15000, more preferably in the range of 5000 to 10000. The number average molecular weight can be measured by gel permeation chromatography.
[0076] The hydroxyl value of the polyester having both an aromatic structure and a polyether structure is preferably 0.2 to 100, more preferably 0.5 to 80. When the Mn and hydroxyl values of the polyester are within the above ranges, the development resistance of the exposed portion and the developability of the unexposed portion are improved, and excellent resolution can be obtained. A curable resin composition having excellent resistance to solder heat and surface hardness as a cured product can also be obtained.
[0077] [Other ingredients]
[0078] Examples of other components include known additives generally used in curable resin compositions, such as inorganic fillers, organic fillers, colorants, organic solvents, thermosetting catalysts, photoinitiator aids, cyanate compounds, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper damage inhibitors, antioxidants, rust inhibitors, thickeners such as fine powdered silica, organic bentonite, and montmorillonite, silicone-based, fluorine-based, polymer-based defoamers and / or leveling agents, imidazole-based, thiazole-based, triazole-based silane coupling agents, phosphinates, phosphate ester derivatives, phosphazene compounds, and other phosphorus compounds, and flame retardants.
[0079] As the inorganic filler, known materials can be used, and one type may be used alone or two or more types may be used in combination.
[0080] Specific examples of inorganic fillers include titanium oxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, fly ash, silicon dioxide (natural silicon dioxide or synthetic silicon dioxide), kaolin, calcium oxide, magnesium oxide, zinc oxide, barium sulfate, aluminum oxide, talc, mica, hydrotalcite, boehmite, calcium hydroxide, wollastonite, potassium titanate, barium titanate, magnesium sulfate, calcium sulfate, sepiolite, copper, iron, carbon black, aluminum oxide, zirconium oxide, antimony oxide, lead white, zinc hydroxide, zinc sulfide, lead titanate, aluminum nitride, silicon nitride, titanium nitride, diamond powder, zirconium silicate, mica Powder, lead sulfate, cerium fluoride, cerium oxide, aluminum phosphite, aluminum silicate, magnesium silicate, calcium silicate, clay, calcined talc, magnesium phosphate, xonotlite, boron nitride, aluminum borate, silica balls, glass flakes, glass balls, amorphous silica, crystalline silica, fused silica, spherical silica, ironmaking slag, iron oxide, iron-silicon-aluminum, aluminum-nickel-cobalt magnets, various ferrites and other magnetic powders, cement, glass powder, dehydrated sludge, Neuburg silica, diatomaceous earth, antimony trioxide, magnesium oxysulfate, hydrated aluminum, hydrated gypsum, alum, phosphorus-containing metal salts such as aluminum phosphite, etc.
[0081] The inorganic filler is preferably silica, barium sulfate or talc from the viewpoint of coating properties, adhesion and chemical resistance, and more preferably silica from the viewpoint of thermal dimensional stability.
[0082] The average particle size of the inorganic filler is not particularly limited as long as it is a particle size that can be used as an inorganic filler. The preferred average particle size is as follows: the average particle size obtained by the volume average particle size distribution measurement result measured by a laser diffraction particle size distribution measuring device is 0.1 μm to 30 μm, and more preferably 0.1 μm to 10 μm.
[0083] The amount of the inorganic filler is preferably 5 to 350 parts by mass, more preferably 10 to 300 parts by mass, and further preferably 30 to 250 parts by mass, based on nonvolatile components, relative to 100 parts by mass of the carboxyl-containing resin. By setting it within this range, a cured product having excellent heat resistance and physical strength can be obtained.
[0084] As the organic solvent, a known organic solvent can be used. In addition, the organic solvent may be used alone or in combination of two or more.
[0085] Specific examples of organic solvents include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, naphtha, and solvent naphtha; and the like.
[0086] The organic solvent is generally used for the purpose of preparing a composition, forming a dry film, adjusting the viscosity when applying to a printed circuit board, etc. Therefore, the content of the organic solvent can be appropriately changed according to the purpose.
[0087] <How to use the curable resin composition>
[0088] Next, as an example of the method of using the curable resin composition of the present invention, a method of forming a dry film and a method of forming a cured product of the curable resin composition on a printed circuit board will be described.
[0089] [Dry film formation method]
[0090] A dry film is generally obtained by performing a coating process and a drying process. Each process is described below.
[0091] (Coating process)
[0092] The curable resin composition is adjusted in viscosity with an organic solvent as necessary, and is applied to a support film (hereinafter also referred to as a "carrier film") at a desired thickness.
[0093] As the support film, a plastic film such as a polyester film such as polyethylene terephthalate, a polyimide film, a polyamide-imide film, a polypropylene film, a polystyrene film, or the like is preferably used.
[0094] The thickness of the support film can be set to, for example, a range of 10 to 150 μm.
[0095] Examples of the coating method include a comma coater, a knife coater, a lip coater, a rod coater, a squeeze coater, a reverse coater, a transfer roll coater, a gravure coater, and a spray coater.
[0096] The coating film thickness can be appropriately set, for example, so that the film thickness after drying becomes within a range of 3 to 100 μm, preferably 5 to 40 μm.
[0097] (Drying process)
[0098] The organic solvent contained in the curable resin composition applied on the support film is volatilized and dried to form a resin layer (dried coating film).
[0099] Examples of the drying means include a hot air circulation drying furnace, an IR furnace, a hot plate, and a convection oven.
[0100] The drying conditions include, for example, a drying temperature of 50 to 130° C. and a drying time of 1 to 30 minutes.
[0101] A removable protective film (hereinafter also referred to as “cover film”) may be laminated on the surface of the resin layer formed on the support film for the purpose of preventing dust from adhering to the surface.
[0102] As the protective film, when the protective film is peeled off, the adhesive force between the resin layer and the protective film is smaller than the adhesive force between the resin layer and the support film. As the protective film, for example, polyethylene film, polytetrafluoroethylene film, polypropylene film, surface-treated paper, etc. can be used.
[0103] [Method for Forming Cured Product]
[0104] The cured product is generally obtained by performing a resin layer forming step, an exposure step, a development step, and a thermal curing step. Each step is described below.
[0105] (Resin layer forming step)
[0106] The curable resin composition is adjusted in viscosity with an organic solvent as needed and applied to a substrate such as a printed circuit board in a desired thickness. Then, the organic solvent contained in the curable resin composition applied to the substrate is evaporated and dried to form a resin layer on the substrate.
[0107] Examples of the coating method include a screen printing method, a curtain coating method, a spray coating method, and a roll coating method.
[0108] The coating film thickness can be appropriately set, for example, so that the film thickness after drying becomes within a range of 3 to 100 μm, preferably 5 to 40 μm.
[0109] Examples of the drying means include a hot air circulation drying furnace, an IR furnace, a hot plate, and a convection oven.
[0110] The drying conditions include, for example, a drying temperature of 50 to 130° C. and a drying time of 1 to 30 minutes.
[0111] The method of forming the resin layer on a substrate such as a printed circuit board may be a method of laminating the above-mentioned dry film on the printed circuit board and transferring the resin layer provided on the dry film to the printed circuit board.
[0112] (Exposure process)
[0113] The resin layer is irradiated with active energy rays through a photomask having a predetermined exposure pattern formed thereon, thereby selectively exposing the resin layer.
[0114] Examples of the active energy ray irradiation light source include a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultrahigh-pressure mercury lamp, a xenon lamp, and a metal halide lamp.
[0115] Here, the exposure method can be divided into a contact exposure method in which exposure is performed in a state where a photomask and a resin layer are in contact, and a non-contact exposure method in which exposure is performed in a state where a photomask and a resin layer are not in contact.
[0116] In the contact exposure method, the resolution is high because the photomask is in contact with the resin layer. On the other hand, when the photomask is removed after exposure, the resin layer adheres to the photomask, contaminating the photomask or causing abnormal stop of the automatic exposure machine, which sometimes deteriorates the continuous productivity. In the non-contact exposure method, the distance between the photomask and the resin layer is far, so the continuous productivity is high, but on the other hand, the resolution tends to be low.
[0117] The resin layer obtained by using the curable resin composition of the present invention can be used in either the non-contact exposure method or the contact exposure method. The curable resin composition of the present invention has excellent dryness to touch and can therefore be preferably used in the contact exposure method.
[0118] (Development Process)
[0119] After the exposure step, development is performed using an alkaline aqueous solution to remove unexposed portions of the resin layer, thereby performing patterning.
[0120] Examples of the alkaline aqueous solution include aqueous alkaline solutions such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, and amines.
[0121] (Thermosetting process)
[0122] After the development step, the resin layer with the pattern formed thereon is further irradiated with active energy rays and then heat-cured (for example, 100 to 220° C.), or irradiated with active energy rays after heat-curing, or finally processed and cured (formal curing) only by heat-curing, to form a cured product with a specified pattern on a substrate such as a printed circuit board.
[0123] The printed circuit board including the cured product of the curable resin composition of the present invention thus obtained can be used for various applications, and is particularly preferably used for vehicles because it is excellent in heat resistance due to the use of chemical tin plating.
[0124] Example
[0125] Hereinafter, the present invention will be specifically described by showing examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that "parts" in the following are all based on mass unless otherwise specified.
[0126] [raw material]
[0127] The carboxyl group-containing resin A and the polyesters E-1 to E-3 having both an aromatic structure and a polyether structure were prepared by the method described below, and commercially available products were used.
[0128] (A) Carboxyl-containing resin: Carboxyl-containing resin A (non-volatile content 65% by mass, solid content acid value 85 mgKOH / g, weight average molecular weight about 3500)
[0129] (B-1) Photopolymerization initiator: IRGACURE 907 (manufactured by BASF Corporation)
[0130] (B-2) Photopolymerization initiator: Kayacure DETX-S (manufactured by Nippon Kayaku Co., Ltd.)
[0131] (C) Thermosetting compound: N-695 (cresol novolac type epoxy manufactured by DIC Corporation)
[0132] (D) Photopolymerizable monomer: dipentaerythritol hexaacrylate (DPHA)
[0133] (E-1) Polyester having both aromatic structure and polyether structure: Polyester E-1 Number average molecular weight Mn: 3000
[0134] (E-2) Polyester with both aromatic structure and polyether structure: Polyester E-2 Number average molecular weight Mn: 8000
[0135] (E-3) Polyester having both aromatic structure and polyether structure: Polyester E-3 Number average molecular weight Mn: 15000
[0136] Inorganic filler (silicon dioxide): Admafine SO-E2 (manufactured by Admatechs)
[0137] Colorant: Phthalocyanine blue
[0138] Colorant: Chrome Phthalo Yellow
[0139] Curing catalyst 1: dicyandiamide (DICY)
[0140] Curing catalyst 2: melamine
[0141] Defoaming agent: KS-66 (manufactured by Shin-Etsu Silicone Co., Ltd.)
[0142] (Preparation of carboxyl group-containing resin)
[0143] Synthesis Example <Carboxyl group-containing resin A>
[0144] 220 parts by mass of cresol novolac epoxy resin (manufactured by DIC Corporation, registered trademark "EPICLON" N-695, epoxy equivalent: 220) was placed in a four-necked flask equipped with a stirrer and a reflux condenser, and 214 parts by mass of carbitol acetate was added and heated to dissolve. Next, 0.1 parts by mass of hydroquinone as a polymerization inhibitor and 2.0 parts by mass of dimethylbenzylamine as a reaction catalyst were added. The mixture was heated to 95-105°C, 72 parts of acrylic acid were slowly added dropwise, and the reaction was carried out for 16 hours. The reaction product was cooled to 80-90°C, 106 parts by mass of tetrahydrophthalic anhydride were added, the reaction was carried out for 8 hours, and the mixture was taken out after cooling.
[0145] The photosensitive resin having both an ethylenically unsaturated bond and a carboxyl group obtained in this manner had a nonvolatile content of 65% by mass, an acid value of a solid matter of 85 mgKOH / g, and a weight average molecular weight Mw of about 3,500.
[0146] The weight average molecular weight of the obtained resin was measured by high performance liquid chromatography connected to a pump LC-6AD manufactured by Shimadzu Corporation and three columns Shodex (registered trademark) KF-804, KF-803, and KF-802 manufactured by Showa Denko K.K.
[0147] (Preparation of polyester having both aromatic structure and polyether structure)
[0148] Synthesis Example 1 <Polyester E-1 (number average molecular weight: 3000)>
[0149] In a 2-liter four-necked flask, 800 parts by mass of a 6-mol ethylene oxide adduct of bisphenol A, 180 parts by mass of adipic acid, and 0.2 parts by mass of titanium tetraisopropoxide as an esterification catalyst were added and reacted at 220° C. to synthesize polyester E-1.
[0150] Synthesis Example 2 <Polyester E-2 (number average molecular weight: 8000)>
[0151] In a 2-liter four-necked flask, 800 parts by mass of a 6-mol ethylene oxide adduct of bisphenol A, 200 parts by mass of adipic acid, and 0.2 parts by mass of titanium tetraisopropoxide as an esterification catalyst were added and reacted at 220° C. to synthesize polyester E-2.
[0152] Synthesis Example 3 <Polyester E-3 (number average molecular weight: 15000)>
[0153] In a 2-liter four-necked flask, 800 parts by mass of a 6-mol ethylene oxide adduct of bisphenol A, 220 parts by mass of adipic acid, and 0.2 parts by mass of titanium tetraisopropoxide as an esterification catalyst were added and reacted at 220° C. to synthesize polyester E-3.
[0154] (Preparation of curable resin composition)
[0155] The components were preliminarily mixed in a stirrer in the composition (parts by mass) shown in Table 1, and then kneaded in a three-roll mill to prepare a curable resin composition.
[0156] (Preparation of test substrate)
[0157] (1) The curable resin composition prepared in each example and comparative example was applied to the entire surface of a printed circuit board having a circuit formed thereon by screen printing using a 100-mesh polyester screen in a thickness of 20 to 30 μm. The coating was then dried in a hot air circulation drying oven at 80° C. for 30 minutes to prepare a test substrate for a test of dryness to touch.
[0158] (2) Next, a photomask having a line pattern of 30 to 150 μm (at intervals of 10 μm) was placed in close contact with the dried coating film, and ultraviolet light (exposure dose 300 mJ / cm2) was irradiated using an ultraviolet light exposure device (manufactured by ORC Manufacturing Co. Ltd., model HMW-680GW). 2 ), then developed in a 1 mass % sodium carbonate aqueous solution at a pressure of 0.2 MPa for 60 seconds. After that, heat cured in a hot air circulation drying oven at 150°C for 60 minutes, cooled naturally to room temperature, and then developed with a high pressure mercury lamp at 1000 mJ / cm 2 The irradiation was performed to prepare a test substrate for testing resolution, solder heat resistance, and chemical tin plating resistance.
[0159] Using the test substrate thus prepared, dryness to touch, resolution, resistance to soldering heat, and chemical tin plating resistance were evaluated. The test methods and evaluation methods for these evaluations are as follows. The evaluation results are shown in Table 1.
[0160] (1) Dryness to touch:
[0161] On the test substrate, the surface of the coating film after drying was directly touched with a finger, and the dryness to touch was evaluated according to the following criteria.
[0162] ◎: No stickiness at all.
[0163] ○: Slightly sticky.
[0164] ×: There is stickiness.
[0165] (2) Resolution:
[0166] The line pattern of the test substrate was measured using an optical microscope and evaluated based on the following criteria.
[0167] ◎: The residual line width is less than 50 μm.
[0168] ○: The residual line width is less than 100 μm.
[0169] ×: The residual line width is 100 μm or more.
[0170] (3) Resistance to welding heat:
[0171] A rosin-based flux was applied to the test substrate, and the substrate was immersed in a solder bath set at 260° C. for 30 seconds. The test substrate was cleaned with an organic solvent, and then subjected to a peeling test using a cellophane tape, and evaluated based on the following criteria.
[0172] ◎: No appearance change.
[0173] ○: Slight peeling was observed on the cured coating film.
[0174] △: Peeling was observed on the cured coating film.
[0175] ×: The cured coating film floated before the peel test, and solder penetration was observed.
[0176] (4) Chemical tin plating resistance:
[0177] The test substrate was subjected to chemical tin plating according to the process described later. The test substrate was subjected to a change in appearance and a peeling test using a cellophane tape, and the peeling state of the cured film was evaluated according to the following criteria.
[0178] ◎: There was no change in appearance and no peeling of the cured film.
[0179] ○: There was no change in appearance, but the cured film was slightly peeled off.
[0180] ×: Floating of the cured film and mechanization of the plating layer were observed, and peeling of the cured film was large in the peeling test.
[0181] Chemical tinning process:
[0182] 1. Degreasing: The test substrate was immersed in an acidic degreasing liquid (a 20 volume % aqueous solution of Metex L-5B manufactured by Nippon MacDermid Co., Ltd.) at 30° C. for 3 minutes.
[0183] 2. Water washing: Immerse the test substrate in running water for 3 minutes.
[0184] 3. Soft etching: The test substrate was immersed in a 14.3 mass % ammonium persulfate aqueous solution at room temperature for 1 minute.
[0185] 4. Water washing: Immerse the test substrate in running water for 3 minutes.
[0186] 5. Acid immersion: The test substrate was immersed in a 10 volume % sulfuric acid aqueous solution at room temperature for 1 minute.
[0187] 6. Water washing: Immerse the test substrate in running water for 30 seconds to 1 minute.
[0188] 7. Chemical tin plating: The test substrate was immersed in a tin plating solution (manufactured by Atotech Corporation, 73 parts by volume of Stanatec H Plus, 6 parts by volume of SF special acid, 5.5 parts by volume of SFTin solution C, 15.5 parts by volume of Stanatec SN calibration solution, and 0.125 parts by volume of Stanatec Additive C) at 70°C and pH = 1 for 12 minutes.
[0189] 8. Water washing: Immerse the test substrate in running water for 3 minutes.
[0190] [Table 1]
[0191]
[0192] From the evaluation results shown in the above table, it was clearly confirmed that in each of the Examples, a curable resin composition having dryness to touch and resolution and having excellent resistance to solder heat and resistance to chemical tin plating was obtained.
Claims
1. A curable resin composition, characterized in that The invention comprises: (A) a carboxyl group-containing resin, (B) a photopolymerization initiator, (C) a thermosetting compound, (D) a photopolymerizable monomer, and (E) a polyester having both an aromatic structure and a polyether structure, wherein the polyester having both an aromatic structure and a polyether structure is a polyester obtained by reacting an alkylene oxide adduct of bisphenol with a polycarboxylic acid, and the number average molecular weight of the polyester having both an aromatic structure and a polyether structure is more than 5000 and less than 15000, The content of the (E) polyester having both an aromatic structure and a polyether structure is 16 to 50 parts by mass based on 100 parts by mass of the (A) carboxyl group-containing resin in terms of non-volatile matter.
2. A dry film, characterized in that: This is obtained by applying the curable resin composition according to claim 1 on a film and drying it.
3. A solidified product, characterized in that: The curable resin composition according to claim 1 or the curable resin composition constituting the dry film according to claim 2 is obtained by subjecting the curable resin composition to at least one of photocuring and thermal curing.
4. A printed circuit board, characterized in that: A cured product according to claim 3.
Citation Information
Patent Citations
Resist ink composition
JP1989054390B2
Photocurable resin composition
CN102472967A