A three-dimensional pipeline component post-argon arc welding correction method
By tidying the three-dimensional pipeline components after argon arc welding and fixing the pipeline with profiling support and plugs, the problems of inconsistent deformation and flow channel uniformity after welding are solved, shortening the processing cycle and reducing production costs. Improves the stability of traffic debugging.
Patent Information
- Application Number
- CN201910628524.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-07-11
AI Technical Summary
After the argon arc welding, the three-dimensional pipeline components have a long length and thin wall thickness, resulting in large deformation after welding, resulting in inconsistent flow channel uniformity, affecting the stability of flow debugging, and repeated trials are required, which increases manpower and Material consumption.
The three-dimensional pipeline assembly is subject to argon arc welding after calibration method, and the profiling support and plug are used for calibration. By placing the pipeline in the accommodating groove and fixing it with plugs, the stability and uniformity of the pipeline are ensured.
It shortens the processing cycle, reduces production costs, improves the uniformity of the internal flow path of the pipeline assembly, reduces changes in flow debugging data, and improves the stability of debugging data.
Smart Images

Figure CN110560518B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding auxiliary equipment, and in particular relates to a method for correcting the shape of a three-dimensional pipeline component after argon arc welding. Background Art
[0002] Since the three-dimensional pipeline components are long and thin, even if argon arc welding is performed on welding tools, large deformation after welding often occurs. In order to improve the uniformity of the internal flow channel of the three-dimensional pipeline, a three-dimensional pipeline component argon arc welding post-shape correction method is designed. This method solves the problem that the deformation of three-dimensional pipeline components with long length and thin wall after argon arc welding is more obvious.
[0003] Generally, after argon arc welding is performed on the tooling of three-dimensional pipeline components, post-weld calibration is not performed, resulting in inconsistent uniformity of the flow channels inside the pipeline components. Therefore, during flow debugging, the flow debugging data will vary greatly, making it difficult to control the stability of the debugging data. Summary of the invention
[0004] The present invention provides a method for correcting the shape of a three-dimensional pipeline component after argon arc welding, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for correcting the shape of a three-dimensional pipeline component after argon arc welding, comprising the following steps:
[0006] S1. Install the pipeline assembly after argon arc welding on the profiling tool for profiling; the profiling tool includes a profiling support for profiling the pipeline assembly, the profiling support is provided with a receiving groove that matches the pipeline assembly, and also includes a support seat A and a support seat B that support the profiling support, and the support seat A and the support seat B are both provided with a plug that matches the pipeline assembly;
[0007] S2. Place the middle section of the pipeline in the receiving tank, tighten the pipe joints with plugs at both ends of the pipeline, and clamp the plugs at both ends on the support seat A and the support seat B respectively;
[0008] S3. After fixing for 30 seconds, take it off.
[0009] Preferably, the plug includes a sliding portion and a fixing rod, the sliding portion and the fixing rod are fixedly connected, and limiting grooves are provided on the support seat A and the support seat B, and the sliding portion is slidably connected to the inner wall of the limiting groove.
[0010] Preferably, the fixing rod is tapered, and the small-diameter end of the fixing rod is located at an end away from the sliding-in portion.
[0011] Preferably, the contoured support is made of clay, and a hard plastic is fixed to an outer wall of the contoured support away from the accommodating groove.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] Since three-dimensional pipeline components are generally not calibrated after argon arc welding on tooling, the uniformity of the internal flow channels of the pipeline components is inconsistent. Therefore, during flow debugging, the flow debugging data will vary greatly, making it difficult to control the stability of the debugging data, resulting in the need to repeat the subsequent flow debugging test many times, wasting unnecessary manpower and material resources. Therefore, after welding, the pipeline is placed in the receiving groove of the contoured support for thirty seconds to fix the pipeline. The above method can shorten the processing cycle and reduce production costs; it can also improve the problem of inconsistent uniformity of the internal flow channels of the pipeline after argon arc welding of the pipeline component. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0015] Figure 1 It is a structural schematic diagram of the present invention;
[0016] Figure 2 It is a schematic diagram of the structure of the plug in the present invention;
[0017] Figure 3 It is a schematic structural diagram of the contoured support member in the present invention.
[0018] In the figure: 1, support seat A; 101, limiting groove; 2, contoured support member; 201, accommodating groove; 3, support seat B; 4, plug; 41, sliding part; 42, fixing rod. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] See also Figure 1-3 The present invention provides the following technical solution: a method for correcting the shape of a three-dimensional pipeline component after argon arc welding, comprising the following steps:
[0021] S1. Install the pipeline assembly after argon arc welding on the profiling tool for profiling; the profiling tool includes a profiling support 2 for profiling the pipeline assembly, the profiling support 2 is provided with a receiving groove 201 that matches the pipeline assembly, and also includes a support seat A1 and a support seat B3 that support the profiling support 2, and the support seat A1 and the support seat B3 are both provided with a plug 4 that matches the pipeline assembly;
[0022] S2, placing the middle section of the pipeline in the receiving groove 201, tightening the pipe joints with plugs 4 at both ends of the pipeline, and clamping the plugs 4 at both ends on the support seat A1 and the support seat B3 respectively;
[0023] S3. After fixing for 30 seconds, take it off.
[0024] In this embodiment: according to different production batches, before mass production, a thick-walled three-dimensional pipeline is simulated and produced, and then the thick-walled three-dimensional pipeline is welded, and then a contoured support 2 is made according to the three-dimensional pipeline. During mass production, the produced thin-walled three-dimensional pipelines are clamped in the receiving groove 201 in the contoured support 2 for profiling. The tooling is used to perform profiling on pipeline components with longer lengths and thinner walls after argon arc welding to improve the uniformity of the internal flow channel of the pipeline component.
[0025] Specifically, the plug 4 includes a sliding portion 41 and a fixing rod 42, the sliding portion 41 and the fixing rod 42 are fixedly connected, and a limiting groove 101 is provided on the support seat A1 and the support seat B3, and the sliding portion 41 is slidably connected to the inner wall of the limiting groove 101; when the intermediate pipeline is placed in the contoured support member 2, the fixing rod 42 of the plug 4 is then clamped at both ends of the pipeline, and then clamped in the limiting groove 101 provided on the support seat A1 and the support seat B3 through the sliding portion 41.
[0026] Specifically, the fixing rod 42 is tapered, and the small-diameter end of the fixing rod 42 is located at the end away from the sliding portion 41 ; since the fixing rod 42 is tapered, it can adapt to pipelines with different inner diameters.
[0027] Specifically, the profiling support 2 is made of clay, and a hard plastic is fixed to the outer wall of the profiling support 2 on one side away from the receiving groove 201; the clay sculpture is convenient for profiling, and the clay sculpture is resistant to high temperature, and the hard plastic fixed on the outer wall increases the reliability of the clay sculpture.
[0028] Usage process: according to different production batches, before mass production, simulate the production of a thick-walled three-dimensional pipeline, then weld the thick-walled three-dimensional pipeline, and then make a contour support 2 according to the three-dimensional pipeline. During mass production, the thin-walled three-dimensional pipelines are clamped in the receiving groove 201 in the contour support 2 for calibration. The tooling is used to calibrate the pipeline components with longer lengths and thinner walls after argon arc welding to improve the uniformity of the internal flow channel of the pipeline components. First, the pipeline components after argon arc welding are installed on the three-dimensional pipeline component argon arc welding calibration tooling for calibration; then the middle section of the pipeline is placed in the accommodating groove 201, and the two ends of the pipeline are respectively tightened with plugs 4 to the pipe joints, and the plugs 4 at both ends are respectively clamped on the support seat A1 and the support seat B3; then, after fixing for 30 seconds, it is taken down, which has the following advantages:
[0029] First, the above method can shorten the processing cycle and reduce production costs;
[0030] Secondly, it can improve the problem of inconsistent uniformity of the flow channel inside the pipeline after argon arc welding of the pipeline components.
[0031] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for correcting the shape of a three-dimensional pipeline component after argon arc welding, characterized in that: The following steps are involved: S1. After the argon arc welding, the pipeline assembly is mounted on a profiling tool for profiling; the profiling tool comprises a profiling support (2) for profiling the pipeline assembly, the profiling support (2) is provided with a receiving groove (201) for cooperating with the pipeline assembly, and also comprises a support seat A (1) and a support seat B (3) for supporting the profiling support (2), and the support seat A (1) and the support seat B (3) are both provided with a plug (4) for cooperating with the pipeline assembly; S2, placing the middle section of the pipeline in the receiving groove (201), tightening the pipe joints with plugs (4) at both ends of the pipeline, and clamping the plugs (4) at both ends on the support seat A (1) and the support seat B (3) respectively; S3. After fixing for 30 seconds, take it off.
2. A method for correcting the shape of a three-dimensional pipeline assembly after argon arc welding according to claim 1, characterized in that: The plug (4) comprises a sliding portion (41) and a fixing rod (42), wherein the sliding portion (41) and the fixing rod (42) are fixedly connected, and a limiting groove (101) is provided on both the support seat A (1) and the support seat B (3), and the sliding portion (41) is slidably connected to the inner wall of the limiting groove (101).
3. A method for correcting the shape of a three-dimensional pipeline assembly after argon arc welding according to claim 2, characterized in that: The fixing rod (42) is tapered, and the small-diameter end of the fixing rod (42) is located at an end away from the sliding-in portion (41).
4. A method for correcting the shape of a three-dimensional pipeline assembly after argon arc welding according to claim 1, characterized in that: The contoured support member (2) is made of clay, and a hard plastic is fixed to the outer wall of the contoured support member (2) on a side away from the containing groove (201).
Citation Information
Patent Citations
Apparatus for pipe end sizing and method for pipe end sizing
CN101410199A
Device and method for rectifying hollow thin-walled castings
CN105268771A
Forming method for precisely twisting metal elbow pipe
CN106944514A
Shape correcting method and tool for large length-diameter ratio ultra-thin wall stainless steel cylindrical piece
CN109433864A
Thin wall machine casket welding deformation's correction instrument
CN206952398U