A method and device for preparing aluminum-magnesium-aluminum composite plate
Through the preparation method of aluminum-magnesium-aluminum composite plates, the combination of concave and convex extrusion dies is used to solve the problems of poor corrosion resistance of magnesium alloys and complex aluminum alloy processing, achieving lightweight, high strength and good corrosion resistance. The preparation of aluminum-clad magnesium composite materials simplifies the processing process and improves the strength of the material and industrial production capabilities.
Patent Information
- Application Number
- CN201911312044.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-12-18
AI Technical Summary
Magnesium alloys have poor corrosion resistance, which limits their wide application. The oxide film of aluminum alloys can prevent further oxidation but is complex to process. It is difficult to effectively combine the advantages of both to prepare lightweight, high-strength, and good corrosion-resistant structural materials.
Using the preparation method of aluminum-magnesium-aluminum composite plates, the aluminum alloy and magnesium alloy are homogenized respectively through a device composed of a concave blank extrusion die and a convex blank extrusion die to form a "T" shape and an "I" shape. The blanks of the cavity are rolled after stacking to reduce grease removal and oxide layer treatment, enhance bonding force and improve composite strength.
It achieves the efficient preparation of aluminum-clad magnesium composite materials, reduces interface defects, enhances the three-dimensional composite area and strength of the composite materials, simplifies the mold structure and operation, reduces the cost, and improves the plastic deformation ability of the plate through the heating device, which is suitable for Industrial production.
Smart Images

Figure CN110842045B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of processing metal composite materials, and in particular relates to a method and a device for preparing an aluminum-magnesium-aluminum composite plate. Background Art
[0002] Magnesium alloy is the lightest structural metal with high strength, high rigidity, good damping, machinability, thermal conductivity, high absorption of vibration and impact, strong electromagnetic shielding ability, abundant resources, easy recycling, etc. However, its corrosion resistance is poor, which hinders the widespread application of magnesium alloy to a certain extent. Aluminum alloy has the characteristics of low density, high specific strength, good thermal conductivity, easy forming, and 100% recycling. Since a dense and stable oxide film is easily formed on the surface of aluminum alloy, it can prevent further oxidation of the internal metal and thus has good corrosion resistance. Aluminum and magnesium are both light metal materials. Due to their high specific strength and specific stiffness, they show more and more extensive application prospects in the manufacturing fields of automobiles, rail transportation, weapons and equipment, aerospace, etc. Aluminum-magnesium composite materials can take into account the advantages of both, thereby preparing lightweight, high-strength, and corrosion-resistant structural materials. Summary of the invention
[0003] The object of the present invention is to provide a method and device for preparing an aluminum-magnesium-aluminum composite plate.
[0004] The technical solution of the present invention is:
[0005] A preparation device for an aluminum-magnesium-aluminum composite plate material, consisting of a concave billet extrusion die and a convex billet extrusion die, wherein the two sets of dies are each composed of an extrusion head, an upper module, a lower module, a heating device, a temperature measuring device, and a fastening device, wherein the upper module matches the lower module and is fixed by the fastening device, wherein one side of the space formed between the upper module and the lower module matches the extrusion head, and the other side is an extrusion working area, and a heating device and a temperature measuring device are arranged on the upper module and / or the lower module, and wherein the lower module of the concave billet extrusion die has a "T"-shaped forming block, and the convex billet extrusion die has an "I"-shaped cavity.
[0006] A method for preparing an aluminum-magnesium-aluminum composite plate using the above device comprises the following steps:
[0007] (1) Perform homogenization treatment on aluminum alloy and magnesium alloy respectively;
[0008] (2) Using a convex billet extrusion die to extrude an “I” shaped magnesium alloy billet;
[0009] (3) using a concave billet extrusion die to extrude two pieces of aluminum alloy billets with a "T"-shaped cavity;
[0010] (4) Laying together two aluminum alloys to form an I-shaped cavity, and squeezing the I-shaped magnesium alloy billet into the two aluminum alloy billets to obtain a composite billet;
[0011] (5) The composite billet is rolled to obtain an aluminum-magnesium-aluminum composite plate.
[0012] Furthermore, the size of the "I"-shaped magnesium alloy billet formed by extrusion is slightly larger than the size of the "I"-shaped cavity formed by laminating the aluminum alloy.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] 1. The method of the present invention generates a new metal surface by extrusion, which can reduce the steps of removing grease and oxide layer before the common composite method. The generated new metal surface can be more conducive to extrusion and rolling composite, and the bonding force of the composite material is good;
[0015] 2. The size of the “I”-shaped magnesium alloy billet is slightly larger than the size of the “I”-shaped cavity formed by the stacking of aluminum alloys, which can combine the three billets and reduce composite interface defects;
[0016] 3. Realize the three-dimensional composite material, increase the composite area and composite strength of the blank;
[0017] 4. The extrusion die of the present invention has a simple die structure, is easy to operate and has low cost;
[0018] 5. The device of the present invention is provided with a heating device to realize preheating treatment before extrusion and improve the plastic deformation ability of the plate. The temperature of the plate can be collected by a thermocouple and transmitted to an external temperature measuring device for detection, and the collected data is transmitted to an external computer system for temperature control.
[0019] 6. The method of the present invention can prepare large aluminum-clad magnesium plates with strong interface bonding ability and high plate quality through the compounding of extrusion and rolling, and can better realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a preparation flow chart of the present invention, wherein: 1. lower module, 2. heating device, 3. temperature measuring device, 4. fastening device, 5. upper module, 6. extrusion head.
[0021] Figure 2 It is a structural schematic diagram of the lower module of the "T"-shaped extrusion die, wherein 11. "T"-shaped forming block.
[0022] Figure 3 It is a structural schematic diagram of the lower module of the "I"-shaped extrusion die, wherein, 12. "I"-shaped cavity.
[0023] Figure 4 This is a schematic diagram of the "T"-shaped upper blank.
[0024] Figure 5This is a schematic diagram of the "I"-shaped blank. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0026] like Figures 1 to 3 As shown, the device of the present invention is composed of a concave billet extrusion die and a convex billet extrusion die. Both sets of dies are composed of a lower module 1, a heating device 2, a temperature measuring device 3, a fastening device 4, an upper module 5, and an extrusion head 6. The lower module 1 of the concave billet extrusion die has a "T"-shaped forming block 11, and the convex billet extrusion die has an "I"-shaped cavity 12. The upper module 5 matches the lower module 1 and is fixed by the fastening device 4. One side of the space formed between the upper module 5 and the lower module 1 matches the extrusion head 6, and the other side is the extrusion working area. The upper module 5 and / or the lower module 1 are provided with a heating device 2 and a temperature measuring device 3. The aluminum alloy billet with a "T"-shaped cavity prepared as shown in FIG. Figure 4 As shown in (2 pieces), the prepared “I” shaped outward convex magnesium alloy billet is as follows Figure 5 As shown in the figure, the size of the "I" shaped magnesium alloy billet formed by extrusion is slightly larger than the size of the "I" shaped cavity formed by lamination of aluminum alloy.
[0027] Example 1
[0028] A 3 mm thick aluminum-clad magnesium composite sheet was prepared by extrusion-rolling composite of one AZ31 magnesium alloy with an initial thickness of 10 mm and two 7050 aluminum alloy billets with an initial thickness of 8 mm.
[0029] (1) The 7050 aluminum alloy was homogenized at 470°C / 24h, and the AZ31 magnesium alloy was homogenized at 415°C / 15h;
[0030] (2) starting the heating device 2, raising the temperature of the concave billet extrusion die to 420° C., and using the concave billet extrusion die with a “T”-shaped forming block 11 and a height of 5 mm to extrude two concave 7050 aluminum alloy billets of the composite billets;
[0031] (3) starting the heating device 2, raising the temperature of the convex billet extrusion die to 400° C., and using the convex billet extrusion die with an “I”-shaped cavity 12 and a height of 10 mm to extrude a composite billet of an outer convex AZ31 magnesium alloy billet;
[0032] (4) stacking two pieces of 7050 aluminum alloy to form an I-shaped cavity, and squeezing the convex AZ31 magnesium alloy billet obtained by extrusion into the concave 7050 aluminum alloy billet to obtain a composite billet;
[0033] (5) The composite billet is preheated to 400°C and kept at this temperature for 30 minutes, and the composite billet is rolled to prepare an aluminum-clad magnesium composite sheet.
[0034] Example 2
[0035] A 3 mm thick aluminum-clad magnesium composite sheet was prepared by extrusion-rolling a piece of AZ31 magnesium alloy with an initial thickness of 8 mm and two pieces of 2519 aluminum alloy billets with an initial thickness of 8 mm.
[0036] (1) 2519 aluminum alloy was homogenized at 530℃ / 12h, and AZ31 magnesium alloy was homogenized at 415℃ / 15h;
[0037] (2) starting the heating device 2, raising the temperature of the concave billet extrusion die to 420° C., and using the concave billet extrusion die with a “T”-shaped forming block 11 and a height of 4 mm to extrude two composite billets of an inner concave 2519 aluminum alloy billet;
[0038] (3) starting the heating device 2, raising the temperature of the convex billet extrusion die to 400° C., and using the convex billet extrusion die with an “I”-shaped cavity 12 and a height of 8 mm to extrude a composite billet of an outer convex AZ31 magnesium alloy billet;
[0039] (4) stacking two pieces of 2519 aluminum alloy to form an I-shaped cavity, and squeezing the convex AZ31 magnesium alloy billet obtained by extrusion into the concave 2519 aluminum alloy billet to obtain a composite billet;
[0040] (5) The composite billet is preheated to 420°C and kept at this temperature for 30 minutes, and the composite billet is rolled to prepare an aluminum-clad magnesium composite sheet.
Claims
1. A method for preparing an aluminum-magnesium-aluminum composite plate, characterized in that: The steps include: (1) Perform homogenization treatment on aluminum alloy and magnesium alloy respectively; (2) Using a convex billet extrusion die to extrude an "I"-shaped magnesium alloy billet; (3) Using a concave billet extrusion die to extrude two pieces of aluminum alloy billets with a "T"-shaped cavity; (4) Laying together two aluminum alloys to form an I-shaped cavity, and squeezing the I-shaped magnesium alloy billet into the two aluminum alloy billets to obtain a composite billet; (5) rolling the composite blank to obtain an aluminum-magnesium-aluminum composite plate; The size of the "I"-shaped magnesium alloy billet formed by extrusion is slightly larger than the size of the "I"-shaped cavity formed by lamination of aluminum alloys; The device used in the preparation method is composed of a concave billet extrusion die and a convex billet extrusion die. The two sets of dies are composed of an extrusion head, an upper module, a lower module, a heating device, a temperature measuring device, and a fastening device. The upper module matches the lower module and is fixed by the fastening device. One side of the space formed between the upper module and the lower module matches the extrusion head, and the other side is the extrusion working area. The upper module and / or the lower module are provided with a heating device and a temperature measuring device. The lower module of the concave billet extrusion die has a "T"-shaped forming block, and the convex billet extrusion die has an "I"-shaped cavity.
Citation Information
Patent Citations
Manufacture method of metal composite board
CN101992568A
Blind way plate
CN105002805A
Laminar composite and preparation method thereof
CN106079739A
Special-shaped interface compounded coin / badge and preparation technology thereof
CN106942855A
Shearing extrusion-rolling composite forming method and device for preparing high-performance panel
CN106984667A