Lead acid battery

By setting the first rib on the negative plate side in the lead-acid battery and controlling the Na concentration, combined with the plate group compression, the problems of lead-acid battery's lead-sulfate accumulation and electrolyte layering in partially charged state are solved, and excellent life span is achieved Performance and charge and discharge efficiency.

CN111279543BActive Publication Date: 2024-11-05GS YUASA INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880070472.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-10-31
Filing Date
2018-10-05
Publication Date
2024-11-05
Estimated Expiration
2038-10-05

AI Technical Summary

Technical Problem

When used in part of the charging state, existing lead-acid batteries are easily caused to accumulation of lead sulfate and electrolyte layering, shorten their lifespan, and increase the risk of penetration and short circuit of the electrolyte in the overdischarge state, affecting charging efficiency.

Method used

By setting the first rib on the negative electrode plate side in the lead-acid battery, and controlling the concentration of Na in the electrolyte is between 0.03 and 0.3 mol/L, combined with appropriate plate group compression, the accumulation of lead sulfate and the electrolyte are suppressed. layering to improve charge and discharge performance.

Benefits of technology

It significantly extends the life performance of lead-acid batteries in partially charged states, reduces the accumulation of lead sulfate, reduces the risk of penetration short circuit, and improves the charge and discharge efficiency and diffusivity of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111279543B_ABST
    Figure CN111279543B_ABST
Patent Text Reader

Abstract

The lead-acid battery comprises: a plate group in which a plurality of positive plates and a plurality of negative plates are stacked with a separator, a battery cell chamber for accommodating the plate group, and an electrolyte. The electrolyte contains 0.03 to 0.3 mol / L of Na. When the two positive plates or the negative plates (end plates) located at the two ends of the plate group are arranged close to the inner wall of the battery cell chamber, the maximum separation distance between the surfaces of the two end plates facing the inner wall of the battery cell chamber is set to L, the total thickness of the positive plates and the negative plates in the plate group is set to d1, the number of inter-electrode spaces in the battery cell chamber is set to N, the total thickness of the separator between the positive plates and the negative plates is set to d2, and the inter-electrode gap W obtained by W=(L-d1) / N-d2 is -0.1 to +0.15 mm. The separator has a first rib on the negative plate side.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lead storage battery. Background Art

[0002] Lead-acid batteries are used in various applications in addition to automotive and industrial applications. Lead-acid batteries include a negative electrode plate, a positive electrode plate, a separator between the negative electrode plate and the positive electrode plate, and an electrolyte. A sulfuric acid aqueous solution is generally used as the electrolyte.

[0003] Patent Document 1 describes a lead acid battery in which an electrolyte solution contains sodium ions in a range of 0.01 to 0.45 mol / L.

[0004] Patent Document 2 describes a lead-acid battery in which an active material layer to which 0.5 wt % to 10 wt % of the positive electrode chemically converted active material is added is disposed near the surface of the positive electrode plate.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2014 / 097522 Pamphlet

[0008] Patent document 2: Japanese Patent Application Publication No. 2000-340252. Summary of the invention

[0009] Lead-acid batteries are sometimes used in an undercharged state called a partial state of charge (PSOC). For example, during charge control or idle stop start (ISS), the lead-acid battery is used under PSOC. Therefore, it is required that the lead-acid battery has excellent life performance (hereinafter referred to as PSOC life performance) in a cycle test under PSOC conditions.

[0010] If the battery is continuously used in the PSOC state, the electrolyte will be stratified, which will promote the softening of the positive electrode active material and the accumulation (sulfation) of lead sulfate in the positive and negative electrode active materials, resulting in a shortened life.

[0011] In addition, if the battery becomes over-discharged and the specific gravity of the electrolyte decreases to near that of water, the solubility of lead increases, and a permeation short circuit is likely to occur. Furthermore, the resistance of the electrolyte increases in the over-discharge state, and charging becomes difficult. In order to prevent these conditions, Na is added to the electrolyte, but this leads to a decrease in charge acceptance in the PSOC state, which easily promotes the accumulation of lead sulfate in the negative electrode (sulfation).

[0012] One aspect of the present invention relates to a lead-acid battery comprising: an electrode group in which a plurality of positive electrode plates and a plurality of negative electrode plates are stacked with a separator interposed therebetween; a battery cell chamber for accommodating the electrode group; and an electrolyte solution, wherein the electrolyte solution contains 0.03 to 0.3 mol / L of Na.

[0013] The positive electrode plate or the negative electrode plate, i.e., the first end plate, located at one end of the electrode plate group is arranged close to one side of the inner side walls facing each other of the battery cell chamber, and the positive electrode plate or the negative electrode plate, i.e., the second end plate, located at the other end of the electrode plate group is arranged close to the other side of the inner side wall. At this time, the maximum separation distance between the surface of the first end plate facing the inner side wall and the surface of the second end plate facing the inner side wall, i.e., the distance between the end plates, is set to L, the total thickness of the positive electrode plate and the negative electrode plate in the electrode plate group is set to d1, the number of regions where the positive electrode plate and the negative electrode plate face each other in the battery cell chamber, i.e., the number of inter-electrode gaps, is set to N, the total thickness of one of the separators between the positive electrode plate and the negative electrode plate is set to d2, and the inter-electrode gap W obtained by the following formula is -0.1 to +0.15 mm.

[0014] W={(L-d1) / N}-d2,

[0015] The separator includes a first rib on the negative electrode plate side.

[0016] In the lead-acid battery, the accumulation of lead sulfate is suppressed, and excellent PSOC life performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a partially cutaway exploded perspective view showing the appearance and internal structure of a lead-acid battery according to one aspect of the present invention. DETAILED DESCRIPTION

[0018] A lead acid battery according to one aspect of the present invention includes: an electrode plate group in which a plurality of positive electrode plates and a plurality of negative electrode plates are stacked with separators interposed therebetween; a battery cell chamber for housing the electrode plate group; and an electrolyte solution containing 0.03 to 0.3 mol / L of Na. In addition, the positive plate or negative plate located at one end of the electrode plate group, i.e., the first end plate, is arranged near one of the inner side walls facing each other in the battery cell chamber, and the positive plate or negative plate located at the other end of the electrode plate group, i.e., the second end plate, is arranged near the other side of the inner side wall. At this time, the maximum separation distance between the surface of the first end plate facing one side of the inner side wall and the surface of the second end plate facing the other side of the inner side wall, i.e., the distance between the end plates is set to L, the total thickness of the positive plate and the negative plate in the electrode plate group is set to d1, the number of regions where the positive plate and the negative plate face each other in the battery cell chamber, i.e., the number of inter-electrode gaps is set to N, and the total thickness of a separator between the positive plate and the negative plate is set to d2. The inter-electrode gap W obtained by the following formula W={(L-d1) / N}-d2 is -0.1 to +0.15 mm. The separator has a first rib on the negative plate side.

[0019] In a lead-acid battery, lead sulfate is generated at both the positive and negative electrodes during discharge, and water is generated at the positive electrode. On the other hand, metallic lead, lead dioxide, and sulfuric acid are generated from lead sulfate and water during charge.

[0020] If the battery is used continuously in an undercharged state, the amount of lead sulfate accumulated will inevitably increase at the end of the PSOC life, so the specific gravity of the electrolyte will decrease. The decrease in the specific gravity of the electrolyte is particularly significant during overdischarge. In addition, if the electrolyte is not sufficiently stirred during charging, a difference in sulfuric acid concentration (stratification) will occur between the upper and lower parts of the electrolyte. If the battery is used continuously in such an environment, sulfation will proceed in the lower part of the electrolyte where the specific gravity is high.

[0021] Adding Na to the electrolyte has the effect of suppressing permeation short circuit and improving the charge recovery from overdischarge. On the other hand, it is known that adding Na will reduce the charge acceptance and easily promote the accumulation of lead sulfate in the negative electrode (sulfation).

[0022] However, the inventors of the present application have found that accumulation of lead sulfate can be suppressed by appropriately applying pressure to the electrode plate group. This is believed to be because expansion of the negative electrode material (negative electrode active material) is mechanically suppressed.

[0023] The degree of compression of the electrode plate group can be evaluated using the inter-electrode gap W represented by the following formula.

[0024] (Inter-electrode gap W) = {(distance between end plates L) - (total thickness of positive and negative plates d1)} / (number of inter-electrode gaps N) - (total thickness of one separator d2)

[0025] Here, the total thickness d1 of the positive and negative plates is the sum of the total thickness of the positive plates that constitute the plate group and the total thickness of the negative plates that constitute the plate group. It should be noted that when the number of positive plates or negative plates in the battery cell chamber exceeds 10, the thickness of the positive plate or negative plate is measured by measuring the thickness of each plate at 6 locations (three locations on the left and right of the plate divided into three equal parts in the height direction) with a caliper, and averaging the measured values ​​of the 10 plates. The total thickness of the positive plate or negative plate is obtained by multiplying the average value of the thickness of the positive plate or negative plate obtained above by the number of the positive plate or negative plate. When the number of positive plates or negative plates in the battery cell chamber is 10 or less, the thickness of each positive plate or negative plate is measured by the above method, and the total thickness is obtained by summing the thicknesses.

[0026] The number of inter-electrode gaps N is the number of regions where the positive electrode plates and the negative electrode plates face each other in the battery cell chamber. In the case of an electrode group in which the positive electrode plates and the negative electrode plates are alternately stacked, (the number of inter-electrode gaps N) = (the number of positive electrode plates) + (the number of negative electrode plates) - 1.

[0027] When ribs are provided on one or both surfaces of the separator, the total thickness d2 of one separator is a value obtained by adding the height of the ribs on one or both surfaces to the basic thickness of the separator.

[0028] The distance L between the end plates is expressed as the maximum distance between the surface of the first end plate facing the inner wall of the battery cell chamber and the surface of the second end plate facing the inner wall of the battery cell chamber when the positive plate or negative plate (hereinafter, appropriately referred to as the "first end plate") located at one end of the electrode group is arranged close to one of the inner walls of the battery cell chamber facing each other and the positive plate or negative plate (hereinafter, appropriately referred to as the "second end plate") located at the other end of the electrode group is arranged close to the other inner wall. When no rib for adjusting the position of the electrode group is provided in the battery cell chamber and the two end plates are directly in contact with the inner wall of the battery cell chamber without a spacer, the distance L between the end plates is equal to the distance between the two inner walls of the battery cell chamber (that is, the internal dimension of the battery cell chamber).

[0029] Sometimes, ribs for adjusting the position of the electrode group are provided in the battery cell chamber. In this case, the first end plate and / or the second end plate contacts the ribs provided in the battery cell chamber without contacting the inner wall of the battery cell chamber, and faces the inner wall of the battery cell chamber via the ribs provided in the battery cell chamber. In this case, the value obtained by subtracting the height of the ribs provided in the battery cell chamber from the internal dimensions of the battery cell chamber is the distance L between the end plates. When ribs are provided on both inner walls of the battery cell chamber, the heights of the two ribs provided on the two inner walls are added together, and the total value is subtracted from the internal dimensions of the battery cell chamber to obtain the distance L between the end plates.

[0030] Alternatively, although the ribs for adjusting the position of the electrode group are not provided in the battery cell chamber, the electrode plates constituting the first end plate and / or the second end plate are contained in a bag-shaped separator. In this case, the end plate is opposite to the inner wall of the battery cell chamber via the separator. In this case, the value obtained by subtracting the total thickness of the separator (the sum of the rib height of the separator and the base thickness) from the internal dimensions of the battery cell chamber is the distance L between the end plates. When both the first end plate and the second end plate are contained in a bag-shaped separator, the total thickness of the two separators is subtracted to obtain the distance L between the end plates.

[0031] Here, the rib height of the separator refers to the maximum height of the rib provided in a region facing a region where the electrode material of the positive electrode plate or the negative electrode plate exists.

[0032] When ribs for adjusting the position of the electrode plate group are provided in the battery cell chamber and the electrode plates constituting the first end plate and / or the second end plate are accommodated in a bag-shaped separator, the height of the ribs provided in the battery cell chamber and the total thickness of the separator are subtracted from the internal dimensions of the battery cell chamber to obtain the distance L between the end plates. However, there are cases where the ribs (external ribs) provided on the outer surface of the bag-shaped separator contact with the ribs provided in the battery cell chamber or where they do not contact with the ribs provided in the battery cell chamber.

[0033] For example, when the electrode assembly is inserted into the battery cell chamber, the outer ribs of the bag-shaped separator are sometimes arranged to cross the ribs provided in the battery cell chamber. In this case, the ribs provided in the battery cell chamber contact the outer ribs of the bag-shaped separator. In this case, the distance L between the end plates is a value obtained by subtracting the height of the ribs provided in the battery cell chamber and the total thickness of the separator (including the height of the inner ribs and the outer ribs) from the internal dimensions of the battery cell chamber.

[0034] On the other hand, it is considered that there is also the following situation: when the electrode group is inserted into the battery cell chamber, the outer ribs of the bag-shaped separator are arranged in a manner that does not cross the ribs provided in the battery cell chamber but is embedded in the gap between the ribs provided in the battery cell chamber. In this case, the ribs provided in the battery cell chamber do not contact the outer ribs of the bag-shaped separator, but contact the base surface of the bag-shaped separator. In this case, the distance L between the end plates is obtained by subtracting the height of the ribs provided in the battery cell chamber and the base thickness of the separator from the internal dimensions of the battery cell chamber, and then subtracting the height of the inner ribs when the ribs (inner ribs) are provided on the inner surface of the bag-shaped separator.

[0035] That is, the inter-electrode gap W is represented by W={(L-d1) / N}-d2, and when the first end plate and the second end plate at the two ends of the electrode group are arranged as close to the two side walls of the battery cell chamber as possible in a manner that the separation distance between the end plates is maximized, the size of the gap in which the positive electrode plate and the negative electrode plate excluding the end plates can move freely in the battery cell chamber is represented as the gap corresponding to the area where the positive electrode plate and the negative electrode plate are opposite. When the inter-electrode gap W is negative, it means that pressure has been applied to the positive and negative plates since the beginning of the manufacture of the lead-acid battery. In addition, even when the inter-electrode gap W is positive, pressure may be applied because the electrode plates expand as the battery is used.

[0036] By applying pressure to the electrode group, the accumulation of lead sulfate can be suppressed. However, on the other hand, by applying pressure to the electrode group, the diffusivity of the electrolyte near the negative electrode is reduced, so there is a tendency for the charge and discharge performance to decrease. If it is not possible to ensure sufficient space between the negative plate and the separator by pressure, sulfuric acid cannot be fully diffused during discharge, and the specific gravity of the electrolyte near the negative electrode is likely to decrease, which can easily lead to a decrease in discharge performance. In addition, during charging, the sulfuric acid released from the negative plate is hindered from diffusing to the separator, and the high concentration of sulfuric acid is retained near the negative electrode, which can easily lead to a decrease in charging efficiency.

[0037] The rib (the first rib) provided on one side of the negative plate ensures a space for maintaining the electrolyte between the negative plate and the separator even under pressure. Thus, the diffusibility of the electrolyte near the negative electrode is maintained even under pressure, and the reduction in charge and discharge performance is suppressed. During discharge, the specific gravity of the electrolyte near the negative electrode is suppressed from decreasing, and the reduction in discharge performance is suppressed. In addition, during charging, the sulfuric acid released from the negative plate can diffuse into the space between the negative plate and the separator, and the specific gravity of the electrolyte near the negative electrode is reduced, thereby improving the charging efficiency.

[0038] Furthermore, the first rib provided on the negative electrode plate improves the diffusibility of the electrolyte, thereby synergistically suppressing the accumulation of lead sulfate. As a result, a lead storage battery having excellent PSOC life performance can be realized.

[0039] As the Na content (concentration) in the electrolyte increases, lead sulfate tends to accumulate, but by providing the first rib and appropriately compressing the electrode group, the accumulation of lead sulfate can be suppressed. If the Na content is 0.3 mol / L or less, the accumulation of lead sulfate can be maintained at a low level, and the reduction in discharge performance can be suppressed. On the other hand, from the perspective of ensuring charge recovery and resistance to penetration short circuits from an overdischarge state, the Na content is preferably 0.02 mol / L or more, and more preferably 0.03 mol / L or more. According to one aspect of the present invention, by providing the first rib, penetration short circuits can be suppressed even with a low Na content of about 0.02 mol / L. Therefore, from the perspective of suppressing the accumulation of lead sulfate and penetration short circuits and obtaining excellent PSOC life performance, the Na content in the electrolyte is preferably 0.02 to 0.3 mol / L, and more preferably 0.03 to 0.3 mol / L.

[0040] In addition, the electrolyte may contain Al, Li and other alkali metal ions or alkaline earth metal ions in addition to Na. The sulfuric acid compounds of these metal ions are more soluble than lead sulfate, and since these metal ions are present in the electrolyte, lead ions are difficult to dissolve. Therefore, the inhibitory effect of permeation short circuit is obtained.

[0041] It should be noted that the content of Na or other metal ions in the electrolyte is obtained by decomposing a fully charged lead-acid battery that has undergone chemical conversion, extracting the electrolyte, and performing inductively coupled plasma (ICP) emission analysis. More specifically, atomic absorption spectrometry is performed using an ICP emission spectrometer (manufactured by Shimadzu Corporation, ICPS-8000), and the concentration of metal ions is obtained using a standard curve.

[0042] The inter-electrode gap W is preferably -0.1 to +0.15 mm. By making the inter-electrode gap W less than 0.15 mm, the accumulation of lead sulfate caused by compression can be inhibited. On the other hand, as the inter-electrode gap W is reduced, the compression is increased, and the discharge characteristics deteriorate. In addition, it becomes difficult to insert the electrode group into the battery cell chamber. From the perspective of maintaining the discharge characteristics and easily inserting the electrode group into the battery cell chamber, the inter-electrode gap W is preferably greater than -0.1 mm.

[0043] According to one embodiment of the present invention, by making the electrolyte contain 0.03 to 0.3 mol / L of Na, the interelectrode gap W is -0.1 to +0.15 mm, and further providing a first rib on one side of the negative electrode plate, the accumulation of lead sulfate is significantly suppressed, and a lead-acid battery with excellent charge and discharge characteristics can be achieved.

[0044] The separator has a first rib provided on the negative plate side. The first rib inhibits the separator from being in close contact with the negative plate. Due to the first rib, the diffusivity of the electrolyte near the negative plate is improved, thereby suppressing the decrease in specific gravity of the electrolyte near the negative plate during discharge. In addition, during charging, the increase in specific gravity of the electrolyte near the negative plate is suppressed. As a result, the charging efficiency is improved. In addition, in addition to the effect brought about by the compression of the plate group, the accumulation of lead sulfate is synergistically suppressed, thereby improving the PSOC life performance.

[0045] The separator may further include a second rib disposed on the positive electrode plate side. The second rib inhibits the separator from being closely attached to the positive electrode plate. The second rib can be used to improve the diffusivity of the electrolyte near the positive electrode plate and inhibit oxidation degradation of the separator, thereby further improving the PSOC life performance.

[0046] The separator can be in the shape of a bag. When a bag-shaped separator is used, although the electrolyte is easily retained, the diffusivity of the electrolyte in the separator is improved by providing the first rib and the second rib, which can further improve the PSOC life performance. Since the positive electrode generates water during discharge, the change in the specific gravity of the electrolyte is greater than that near the negative plate. However, when the bag-shaped separator accommodates the positive plate, the diffusivity of the electrolyte near the positive plate is improved, and it is easy to suppress the stratification of the electrolyte. On the other hand, when the bag-shaped separator accommodates the negative plate, it is easy to suppress the short circuit caused by the elongation of the positive grid. In addition, by forming the first rib in the bag, the diffusivity of the electrolyte near the negative plate is improved, and stratification is easy to suppress.

[0047] In addition, the negative plate contains a negative electrode material, and the negative electrode material may contain conductive carbon particles. Adding carbon to the electrode material has the effect of inhibiting the accumulation of lead sulfate and improving the life performance of PSOC. On the other hand, when the carbon particles contain first carbon particles having a particle size of less than 32 μm, and the first carbon particles contain second carbon particles having a particle size smaller than the average pore diameter of the separator, the carbon particles flowing into the electrolyte block the pores of the separator, which may lead to a decrease in battery performance (for example, low temperature and high rate performance). However, by providing a first rib on the negative plate side, the pores of the separator are not easily blocked by carbon particles, which can inhibit performance degradation. The content of the first carbon particles in the negative electrode material is preferably 0.2 mass % to 2 mass %.

[0048] The lead-acid battery may include a fiber mat between the positive plate and the negative plate. When the fiber mat is provided, the electrode plate is compressed by the fiber mat, so that the electrolyte around the electrode plate becomes less and the diffusivity is also reduced. However, by providing at least the first rib on the negative plate side of the separator, the electrolyte can be kept near the negative plate even when the fiber mat is provided, and the diffusivity of the electrolyte can be improved.

[0049] In this specification, the fully charged state of a lead-acid battery, in the case of a liquid battery, refers to a state after constant current charging at a current of 0.2CA in a water tank at 25°C until it reaches 2.5V / battery cell, and then further constant current charging at 0.2CA for 2 hours. In addition, in the case of a valve-regulated battery, the fully charged state refers to a state in which constant current constant voltage charging at 0.2CA, 2.23V / battery cell, is performed in an air tank at 25°C, and charging is terminated when the charging current during constant voltage charging reaches less than 1mCA.

[0050] It should be noted that in this specification, 1CA refers to the current value (A) of the same numerical value as the nominal capacity (Ah) of the battery. For example, if the nominal capacity of the battery is 30Ah, 1CA is 30A, and 1mCA is 30mA.

[0051] Hereinafter, a lead acid battery according to an embodiment of the present invention will be described with respect to each main component, but the present invention is not limited to the following embodiment.

[0052] (Isolator)

[0053] The separator has a base portion composed of a microporous membrane, and a rib protruding from one main surface of the base portion. It is more preferred that the separator further has a rib protruding from another main surface of the base portion. The rib protruding from one main surface of the base portion is configured in a manner to be located on the negative plate side. The rib located on the negative plate side is referred to as the first rib. The rib protruding from the other main surface of the base portion is configured on the positive plate side (i.e., opposite to the positive plate). The rib located on the positive plate side is referred to as the second rib. Since the diffusibility of the electrolyte near the negative plate can be improved by the first rib, the PSOC life performance can be further improved, and the penetration short circuit can be suppressed.

[0054] The separator is formed of a polymer material (which is different from a fiber). At least the base portion is a porous sheet, which can also be referred to as a porous membrane. The average pore diameter of the base portion can be regarded as the average pore diameter of the separator. The separator may contain a filler (e.g., a granular filler such as silicon dioxide and / or a fibrous filler) dispersed in a matrix formed by the polymer material. The separator is preferably composed of an acid-resistant polymer material. As such a polymer material, polyolefins such as polyethylene and polypropylene are preferred.

[0055] The average pore diameter of the base portion of the separator is, for example, 0.01 μm to 0.5 μm, or preferably 0.03 μm to 0.3 μm. When the average pore diameter is within such a range, low resistance and excellent short-circuit resistance can be achieved at the same time, which is advantageous.

[0056] The average pore diameter of the separator can be obtained by mercury intrusion. More specifically, the separator is placed in a measuring container, evacuated, and then filled with mercury under pressure. The pore distribution is obtained from the relationship between the pressure at that time and the volume of mercury pressed into the separator, and the average pore diameter is obtained from the pore distribution. The average pore diameter is measured using an automatic mercury intrusion meter (AutoPore IV9505) manufactured by Shimadzu Corporation.

[0057] The average thickness of the base portion is, for example, 100 μm to 300 μm, preferably 150 μm to 250 μm. When the average thickness of the base portion is within such a range, a high capacity is ensured, the first rib is easily ensured, and the height of the second rib as required is ensured.

[0058] The average thickness of the base portion is determined by averaging the thickness of the base portion measured at five locations randomly selected in the cross-sectional photograph of the separator.

[0059] The first rib is formed on the surface of the separator on the side opposite to the negative electrode plate. The height of the first rib is, for example, 0.05 mm or more, preferably 0.07 mm or more. When the height of the first rib is in such a range, the electrolyte becomes easier to diffuse. From the viewpoint of ensuring high capacity, the height of the first rib is, for example, 0.40 mm or less, preferably 0.20 mm or less. These lower limits and upper limits can be arbitrarily combined.

[0060] It should be noted that the height of the first rib refers to the maximum height of the first rib existing in the area opposite to the area where the negative electrode material exists on the negative plate unless otherwise specified. The height of each first rib is the distance from one main surface of the base to the top of the first rib. When the main surface of the base is not a plane, when the separator is laid flat with the first rib side facing upward, the distance from the highest position of one main surface of the base to the highest position of the top of the first rib at the specified position of the first rib is taken as the height of the first rib.

[0061] In one main surface of the base portion, the pattern of the first rib is not particularly limited, and the first rib can be formed randomly, or it can be formed in a stripe shape, a curve shape, a grid shape, etc. From the viewpoint of making it easier for the electrolyte to diffuse, in one main surface of the base portion, it is preferred that a plurality of first ribs are formed in a stripe shape. The orientation of the striped first rib is not particularly limited, for example, a plurality of first ribs can be formed along the height direction and the width direction of the negative electrode plate. The specific gravity of the electrolyte is likely to differ above and below the electrode plate, so from the viewpoint of further improving the diffusibility of the electrolyte, it is preferred that a plurality of first ribs are formed in a stripe shape along the height direction of the negative electrode plate.

[0062] It should be noted that an ear portion for extracting current from the electrode group is usually formed at one end of the negative electrode plate and the positive electrode plate. The vertical direction of the negative electrode plate and the positive electrode plate with the ear portion facing upward is called the height direction of the negative electrode plate and the positive electrode plate. The width direction of the negative electrode plate and the positive electrode plate refers to the direction that is orthogonal to the height direction and crosses the main surface of the negative electrode plate and the positive electrode plate.

[0063] The spacing of the stripe-shaped or grid-shaped first ribs is, for example, 0.3 mm to 10 mm, preferably 0.5 mm to 5 mm. When the separator includes a region where the first rib is formed at a spacing in such a range, it is easy to obtain the effect of improving the diffusivity of the electrolyte near the negative plate. In the separator, it is preferred to form the first rib at such a spacing in the region opposite to the negative plate. For example, it is preferred to form the first rib at such a spacing with more than 70% of the area of ​​the region opposite to the negative plate. The first rib may be formed in an area that is not opposite to the negative plate, such as the end of the separator, or the first rib may not be formed, and a plurality of first ribs may be densely formed (for example, at an average spacing of 0.5 mm to 5 mm).

[0064] It should be noted that the pitch between the first ribs refers to the distance between the tops of the adjacent first ribs (more specifically, the distance between the centers of the adjacent first ribs in a direction crossing the first ribs).

[0065] The average spacing of the first ribs is obtained by averaging the spacing of the first ribs measured at 10 randomly selected locations. It should be noted that when the first ribs are densely formed in a region not facing the negative electrode plate, the average spacing can be calculated in addition to the region. For this region, the average spacing of the first ribs in the region not facing the negative electrode plate can be calculated in the same manner as described above.

[0066] The second rib is formed on the surface of the separator on one side opposite to the positive plate. The height of the second rib is, for example, 0.3 mm or more, preferably 0.4 mm or more. When the height of the second rib is in such a range, it is easy to suppress the oxidative degradation of the separator. From the viewpoint of ensuring high capacity, the height of the second rib is, for example, 1.0 mm or less, and can be 0.7 mm or less. These lower limits and upper limits can be arbitrarily combined.

[0067] It should be noted that the height of the second rib refers to the maximum height of the second rib existing in the area opposite to the area where the positive electrode material of the positive plate exists, unless otherwise specified. The maximum height of the second rib is obtained according to the situation of the first rib. The height of each second rib is the distance from one main surface of the base portion to the top of the second rib.

[0068] The pattern and orientation of the second rib are not particularly limited, and for example, can be selected from the patterns and orientations described for the first rib. The spacing of the stripe-shaped or grid-shaped second ribs is, for example, 1 mm to 15 mm, preferably 5 mm to 10 mm. When the separator includes an area where the second ribs are formed with a spacing in such a range, the effect of suppressing oxidative degradation of the separator is further improved. In the separator, the second ribs are preferably formed with such a spacing in the area opposite to the positive plate. For example, the second ribs with such a spacing are preferably formed with more than 70% of the area of ​​the area opposite to the positive plate. The second ribs may or may not be formed in areas that are not opposite to the positive plate, such as the ends of the separator, and a plurality of second ribs may be densely formed (for example, with an average spacing of 0.5 mm to 5 mm).

[0069] The pitch of the second ribs refers to the distance between the tops of adjacent second ribs (more specifically, the distance between the centers of adjacent second ribs in a direction crossing the second ribs). The average pitch of the second ribs can be calculated based on the average pitch of the first ribs.

[0070] A sheet-like separator can be sandwiched between the negative plate and the positive plate, and the separator can be placed between the negative plate and the positive plate by accommodating the negative plate or the positive plate with a bag-like separator. When a bag-like separator is used, although the electrolyte becomes difficult to diffuse, the diffusivity is improved by providing the first rib and the second rib. When the negative plate is accommodated with a bag-like separator, the diffusivity of the electrolyte near the negative plate is easily improved by the first rib, and even if the positive collector is elongated, the short circuit caused by the breakage of the separator can be suppressed. When the positive plate is accommodated with a bag-like separator, the stratification of the electrolyte is easily suppressed.

[0071] The separator is obtained, for example, by extruding a resin composition containing a pore former (solid pore former such as polymer powder and / or a liquid pore former such as oil) and a polymer material into a sheet, removing the pore former, and forming pores in the matrix of the polymer material. The ribs can be formed, for example, during extrusion molding, or by extruding with a roller having grooves corresponding to the ribs after molding into a sheet or removing the pore former. When a filler is used, it is preferably added to the resin composition.

[0072] (Electrolyte)

[0073] The electrolyte contains sulfuric acid in an aqueous solution. The electrolyte may be gelled as needed. The electrolyte may contain additives used in lead-acid batteries as needed.

[0074] In the present embodiment, the electrolyte solution contains Na at a concentration of 0.03 to 0.3 mol / L.

[0075] The specific gravity of the electrolyte in a fully charged lead-acid battery at 20°C after chemical conversion is, for example, 1.10 g / cm3 ~1.35g / cm 3 .

[0076] (Positive plate)

[0077] The positive plates of lead-acid batteries are of paste type and clad type.

[0078] The paste-type positive electrode plate comprises a positive electrode collector and a positive electrode material. The positive electrode material is retained in the positive electrode collector. In the paste-type positive electrode plate, the positive electrode material is the substance after the positive electrode collector is removed from the positive electrode plate. The positive electrode collector can be formed in the same manner as the negative electrode collector, and can be formed by casting lead or lead alloy, or processing lead or lead alloy sheets.

[0079] The clad positive plate comprises a plurality of porous tubes, a core metal inserted into each tube, a positive electrode material filled in the tubes into which the core metal is inserted, and a connector connecting the plurality of tubes. In the clad positive plate, the positive electrode material is the substance obtained by removing the tubes, the core metal and the connector from the positive plate.

[0080] As the lead alloy used in the positive electrode collector, Pb-Ca alloy and Pb-Ca-Sn alloy are preferred in terms of corrosion resistance and mechanical strength. The positive electrode collector may have lead alloy layers with different compositions, and the alloy layers may be multiple. Pb-Ca alloy and Pb-Sb alloy are preferably used for the core.

[0081] The positive electrode material contains a positive electrode active material (lead dioxide or lead sulfate) that develops capacity through an oxidation-reduction reaction. The positive electrode material may contain other additives as necessary.

[0082] The non-chemically converted paste-type positive electrode plate is obtained by filling the positive electrode collector with a positive electrode paste, aging, and drying, as in the case of the negative electrode plate. Thereafter, the non-chemically converted positive electrode plate is chemically converted. The positive electrode paste is prepared by kneading lead powder, additives, water, and sulfuric acid.

[0083] The non-chemically converted clad positive electrode plate is formed by filling a tube into which a core metal is inserted with a mixture of an additive and lead powder or lead powder in a slurry form, and connecting a plurality of tubes with a joint.

[0084] (Negative plate)

[0085] The negative plate of a lead-acid battery contains a negative electrode material. Usually, the negative plate of a lead-acid battery is composed of a negative current collector and a negative electrode material. The negative electrode material is a substance after removing the negative current collector from the negative plate. The negative current collector can be formed by casting lead (Pb) or a lead alloy, or by processing lead or lead alloy sheets. As a processing method, for example, a mesh processing and a punching processing can be cited. When a negative grid is used as a negative current collector, it is easy to carry the negative electrode material, so it is preferred.

[0086] The lead alloy used in the negative electrode current collector may be any one of a Pb-Sb alloy, a Pb-Ca alloy, and a Pb-Ca-Sn alloy. These lead or lead alloys may further contain at least one selected from Ba, Ag, Al, Bi, As, Se, Cu, etc. as an additive element.

[0087] The negative electrode material contains a negative electrode active material (lead or lead sulfate) that develops capacity through redox reaction, and may contain a shrinkage preventer, a carbonaceous material such as carbon black, barium sulfate, and other additives as needed.

[0088] Although the negative electrode active material in the charged state is spongy lead, the negative electrode plate that has not been chemically converted is usually made of lead powder.

[0089] The negative electrode material may contain carbon particles as an additive. Carbon particles are generally conductive. Examples of carbon particles include carbon black, graphite, hard carbon, and soft carbon. Examples of carbon black include acetylene black, furnace black, channel black, and lamp black. Graphite may be any carbon material containing a graphite-type crystal structure, and may be artificial graphite or natural graphite. The negative electrode material may contain one of these carbon particles, or may contain two or more of these carbon particles.

[0090] The carbon particles contain first carbon particles having a particle size of less than 32 μm, and preferably the first carbon particles contain second carbon particles having a particle size smaller than the average pore diameter of the separator. The carbon particles contained in the negative electrode material only need to contain at least the first carbon particles, or may contain only the first carbon particles, or may contain the first carbon particles and carbon particles (third carbon particles) having a particle size of 32 μm or more.

[0091] The second carbon particles preferably contain carbon black. Although the second carbon particles such as carbon black easily flow into the electrolyte, even if they flow into the electrolyte, the first rib can prevent the pores of the separator from being clogged by the second carbon particles. In addition, by including the second carbon particles such as carbon black in the first carbon particles, a more uniform conductive network can be easily formed in the negative electrode material.

[0092] The content of the carbon particles in the negative electrode material is, for example, 0.2 mass % to 3.0 mass %, preferably 0.3 mass % to 2.5 mass %. When the content of the carbon particles is within such a range, a high capacity is ensured and the conductive network is easily expanded.

[0093] The ratio of the first carbon particles in the carbon particles (the total amount of carbon particles) contained in the negative electrode material is, for example, 10% by mass or more, preferably 30% by mass or more. The ratio of the first carbon particles in the carbon particles (the total amount of carbon particles) contained in the negative electrode material is 100% by mass or less, and may be 90% by mass or less. These lower limits and upper limits may be combined arbitrarily.

[0094] The content of the first carbon particles in the negative electrode material is preferably, for example, 0.2 mass % to 2 mass %. By using a negative electrode plate having a negative electrode material containing the first carbon particles at such a content and a separator having a first rib, the diffusibility of the electrolyte near the negative electrode plate can be improved, and high PSOC life performance can be ensured. When the content of the first carbon particles in the negative electrode material is 0.2 mass % or more, although the second carbon particles contained in the first carbon particles are easy to flow into the electrolyte during charging and discharging, the presence of the first ribs inhibits the pores of the separator from being blocked by the first carbon particles flowing out. Thus, it is possible to inhibit the reduction of battery performance, such as the reduction of low-temperature high-rate performance. In addition, by making the content of the first carbon particles in the negative electrode material less than 2 mass %, the hardening of the negative electrode paste can be inhibited, and the reduction of the coating or filling properties of the collector can be inhibited. In addition, even under conditions where permeation short circuits are easily caused due to longevity, stratification is reduced by the high diffusibility of the electrolyte, so the occurrence of permeation short circuits can be inhibited. From the viewpoint that the effect of suppressing the reduction of low-temperature high-rate performance brought about by the first rib is obvious, the content of the first carbon particles in the negative electrode material is preferably 0.3% by mass to 2% by mass. In addition, from the viewpoint of suppressing the amount of liquid reduction during charging to a low level, it is also preferred that the content of the first carbon particles in the negative electrode material is 1% by mass or less (for example, 0.2% by mass to 1% by mass or 0.3% by mass to 1% by mass).

[0095] The average particle size a1 of the second carbon particles (for example, carbon black, etc.) contained in the first carbon particles is preferably less than 100 nm, more preferably less than 60 nm, and the lower limit is not particularly limited, preferably more than 10 nm, and can also be more than 20 nm. These upper and lower limits can be combined arbitrarily. When the average particle size of the first carbon particles is in such a range, the first carbon particles easily flow into the electrolyte, making the pores of the separator easy to clog. However, by using an separator having a first rib, the clogging of the pores of the separator can be suppressed, and the reduction of low-temperature high-rate performance can be suppressed.

[0096] The third carbon particles preferably include carbon particles other than carbon black among the above-mentioned carbon particles, and particularly preferably include graphite.

[0097] The ratio R (= a1 / a2) of the average particle size (a1) of the second carbon particles to the average pore diameter (a2) of the separator is preferably 0.8 or less, and more preferably 0.5 or less. When the ratio R is in such a range, the second carbon particles are likely to clog the pores of the separator, but the first rib of the separator can ensure the diffusivity of the electrolyte near the negative plate, and can suppress the clogging of the pores of the separator. Therefore, high PSOC life performance can be ensured, and the reduction of low-temperature high-rate performance can be further suppressed.

[0098] The contents of the carbon particles and the first carbon particles contained in the negative electrode material, and the average particle size of the second carbon particles and the ratio of the second carbon particles can be determined as follows.

[0099] The lead-acid battery that has been chemically converted and fully charged is dismantled, and the negative plate is washed and dried to remove the sulfuric acid component, and then vacuum dried (dried at a pressure lower than atmospheric pressure). Next, the electrode material is taken from the negative plate and crushed. 30 mL of a 60% by mass aqueous nitric acid solution is added to 5 g of the crushed sample, and heated at 70°C to dissolve the lead into lead nitrate. 10 g of disodium ethylenediaminetetraacetate, 30 mL of ammonia water with a concentration of 28% by mass, and 100 mL of water are further added to the mixture, and heating is continued to dissolve the soluble components. Next, the sample recovered by filtration is passed through a sieve with a mesh size of 500 μm to remove larger components such as reinforcing materials, and the components passing through the sieve are recovered as carbon particles.

[0100] When the recovered carbon particles are wet-screened using a sieve with a mesh size of 32 μm, particles that cannot pass through the mesh of the sieve and remain on the sieve are regarded as third carbon particles, and particles that pass through the mesh of the sieve are regarded as first carbon particles. It should be noted that wet screening can refer to JIS Z8815:1994.

[0101] Specifically, the carbon particles are placed on a sieve with a mesh size of 32 μm, and the sieve is gently shaken for 5 minutes while spraying ion exchange water for sieving. The third carbon particles remaining on the sieve are recovered from the sieve by perfusing ion exchange water and separated from the ion exchange water by filtration. The first carbon particles passing through the sieve are recovered by filtering using a membrane filter made of cellulose nitrate (mesh size 0.1 μm). The recovered first carbon particles and third carbon particles are dried at a temperature of 110°C for 2 hours, respectively. As a sieve with a mesh size of 32 μm, a sieve with a nominal mesh size of 32 μm as specified in JIS Z 8801-1:2006 is used.

[0102] The first carbon particles passing through the mesh of the sieve contain many second carbon particles having a smaller primary particle size. As described later, the average particle size of such primary particles is equivalent to the average particle size a1 of the second carbon particles. Such second carbon particles contained in the first carbon particles flow into the electrolyte and become the cause of clogging the pores of the separator because the particle size is smaller than the average pore diameter a2 of the separator.

[0103] The content of the first carbon particles in the negative electrode material is obtained by measuring the mass of the first carbon particles separated according to the above steps and calculating the ratio (mass %) of the mass in 5g of the pulverized sample. The content (mass %) of the carbon particles in the negative electrode material is obtained by adding the ratio of the third carbon particles obtained according to the situation of the first carbon particles and the ratio of the first carbon particles.

[0104] The average particle size a1 of the second carbon particles is determined by randomly selecting 100 primary particles having a primary particle size smaller than the average pore diameter d2 of the separator from an electron microscope photograph of the first carbon particles, measuring the maximum diameter (major axis diameter) of each primary particle, and calculating the average value.

[0105] The ratio of the second carbon particles contained in the first carbon particles can be determined as follows based on the scanning electron microscope (SEM) photograph of the above-mentioned separated first carbon particles. First, in the SEM photograph, select any area of ​​100 μm in length × 100 μm in width. For the carbon particles contained in this area and with clear outer edges of the particles, particles with a primary particle size smaller than the average pore diameter a2 of the separator are regarded as second carbon particles, and particles with a primary particle size greater than the average pore diameter a2 are regarded as first carbon particles other than the second carbon particles. Then, for each carbon particle, the area of ​​the area enclosed by the outer edge of the particle is calculated, and the volume of the particle is converted from the area and the primary particle size of the particle. Then, the total volume of the second carbon particles and the total volume of the first carbon particles other than the second carbon particles are calculated, and the ratio (volume %) of the total volume of the second carbon particles in the total volume of the two is calculated.

[0106] The negative electrode plate can be made by filling the negative electrode collector with a negative electrode paste, aging and drying to produce a non-chemically converted negative electrode plate, and then chemically converting the non-chemically converted negative electrode plate. The negative electrode paste is made by adding water and sulfuric acid to lead powder, an organic shrink-proof agent, and various additives as needed, and kneading them. In the aging process, it is preferred to age the non-chemically converted negative electrode plate at a temperature higher than room temperature and high humidity.

[0107] The chemical conversion can be performed by charging the electrode group while the electrode group including the unconverted negative electrode is immersed in an electrolyte containing sulfuric acid in a battery tank of a lead-acid battery. However, the chemical conversion can also be performed before assembling the lead-acid battery or the electrode group. Spongy lead is generated by the chemical conversion.

[0108] (Fiber Felt)

[0109] The lead-acid battery may further include a fiber mat between the positive electrode plate and the negative electrode plate. When the fiber mat is arranged, the electrode plate is compressed by the fiber mat, and it becomes difficult to keep the electrolyte around the electrode plate. In the above aspect of the present invention, since the first rib is provided on the separator, it is easy to keep the electrolyte near the negative electrode plate, and the high diffusibility of the electrolyte can be ensured.

[0110] The fiber felt is different from the separator and is composed of a sheet-like fiber assembly. As such a fiber assembly, a sheet obtained by interweaving fibers that are insoluble in the electrolyte can be used. Such sheets include, for example, nonwoven fabrics, woven fabrics, knitted fabrics, and the like.

[0111] As the fiber, glass fiber, polymer fiber (polyolefin fiber, acrylic fiber, polyester fiber such as polyethylene terephthalate fiber, etc.), pulp fiber, etc. can be used. Among the polymer fibers, polyolefin fiber is preferred.

[0112] The fiber mat may contain components other than fibers, for example, acid-resistant inorganic powders, polymers as binders, etc. As inorganic powders, silica powder, glass powder, diatomaceous earth, etc. may be used. Among them, the fiber mat is mainly composed of fibers. For example, more than 60% by mass of the fiber mat is formed by fibers.

[0113] The fiber felt only needs to be arranged between the negative plate and the positive plate. Since a separator is also arranged between the negative plate and the positive plate, the fiber felt can be arranged between the negative plate and the positive plate, for example, between the negative plate and the separator and / or between the separator and the positive plate. From the viewpoint of suppressing the stratification of the electrolyte, the fiber felt is preferably arranged in contact with the negative plate. In addition, from the viewpoint of suppressing the softening and shedding of the positive electrode material, the fiber felt is preferably arranged in contact with the positive plate. From the viewpoint of improving the effect of suppressing softening and shedding, the fiber felt is preferably arranged in a state of being pressed against the positive plate, in which case the electrolyte near the negative plate is easily insufficient. In the present embodiment, since the first rib is provided on the surface of the separator on the side opposite to the negative plate, the electrolyte can be ensured to be near the negative plate even when the fiber felt is arranged on the positive plate side.

[0114] Figure 1 2 shows the appearance of an example of a lead storage battery according to an embodiment of the present invention.

[0115] The lead-acid battery 1 includes a battery tank 12 for accommodating a plate group 11 and an electrolyte (not shown). The battery tank 12 is divided into a plurality of battery cell chambers 14 by partition walls 13. Each battery cell chamber 14 accommodates one plate group 11. The opening of the battery tank 12 is closed by a cover 15 having a negative terminal 16 and a positive terminal 17. A liquid port plug 18 is provided on the cover 15 corresponding to each battery cell chamber. When replenishing water, the liquid port plug 18 is removed to replenish the replenishing liquid. The liquid port plug 18 can have the function of discharging the gas generated in the battery cell chamber 14 to the outside of the battery.

[0116] The electrode group 11 is formed by stacking a plurality of negative plates 2 and positive plates 3 respectively with a separator 4 therebetween. Here, a bag-shaped separator 4 for accommodating the negative plates 2 is shown, but the form of the separator is not particularly limited. In the battery cell chamber 14 located at one end of the battery tank 12, the negative electrode shelf 6 in which a plurality of negative plates 2 are connected in parallel is connected to the through connector 8, and the positive electrode shelf 5 in which a plurality of positive plates 3 are connected in parallel is connected to the positive electrode column 7. The positive electrode column 7 is connected to the positive electrode terminal 17 on the outside of the cover 15. In the battery cell chamber 14 located at the other end of the battery tank 12, the negative electrode column 9 is connected to the negative electrode shelf 6, and the through connector 8 is connected to the positive electrode shelf 5. The negative electrode column 9 is connected to the negative electrode terminal 16 on the outside of the cover 15. Each through connector 8 connects the electrode group 11 of the adjacent battery cell chambers 14 in series with each other through the through hole provided in the partition 13.

[0117] [Example]

[0118] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0119] 《Lead-acid battery A1》

[0120] (1) Production of negative electrode plate

[0121] Lead powder, water, dilute sulfuric acid, carbon black, and an organic shrinkage-proofing agent are mixed to obtain a negative electrode paste. The negative electrode paste is filled into the mesh of a Pb-Ca-Sn alloy expanded mesh grid as a negative electrode current collector, aged and dried to obtain a negative electrode plate that is not chemically converted. Sodium lignin sulfonate is used as an organic shrinkage-proofing agent. The carbon black and organic shrinkage-proofing agent are added in an amount adjusted to 0.3% by mass and 0.2% by mass in 100% by mass of the negative electrode material, respectively, and are mixed in the negative electrode paste.

[0122] (2) Production of positive electrode plate

[0123] Lead powder, water and sulfuric acid are kneaded to prepare a positive electrode paste, which is filled into the mesh of a Pb-Ca-Sn alloy expanded grid as a positive electrode current collector, aged and dried to obtain a non-chemically converted positive electrode plate.

[0124] (3) Production of lead-acid batteries

[0125] Each unconverted negative electrode plate is housed in a bag-shaped separator formed of a polyethylene microporous film, and a plate group is formed by 7 unconverted negative electrodes and 6 unconverted positive electrodes corresponding to each battery cell. The separator has a plurality of striped second ribs on the outside of the bag. The separator uses a separator in which the first rib is not provided on the inside of the bag. The plurality of second ribs are formed along the height direction of the positive electrode plate, the height of the second rib is 0.4 mm, and the spacing of the second ribs in the area opposite to the positive electrode plate is 10 mm. In addition, the average thickness of the base portion of the separator is 200 μm. The average pore diameter of the separator is 0.1 μm.

[0126] The electrode group was inserted into a polypropylene battery tank, and the electrolyte was injected. Chemical conversion was performed in the battery tank to assemble a liquid lead-acid battery A1 with a nominal voltage of 2V and a nominal capacity of 30Ah (5 hour rate). As the electrolyte, an aqueous solution containing sulfuric acid with a specific gravity of 1.28 at 20°C was used. The interelectrode gap W was found to be 0.2mm.

[0127] For a fully charged lead-acid battery that has undergone chemical conversion, the average particle size a1 of the second carbon particles (carbon black) contained in the negative electrode material and the average pore diameter a2 of the separator are calculated in the above order. The results are 50 nm and 0.1 μm, respectively, and the ratio R = a1 / a2 is 0.5. The content of the first carbon particles is almost the same as the amount of carbon black added when preparing the negative electrode material. In addition, the average pore diameter of the separator is also almost the same as the average pore diameter of the separator before assembling the battery.

[0128] 《Lead-acid battery A2~A26》

[0129] As an electrolyte, sodium sulfate (Na2SO4) was added to the above aqueous solution containing sulfuric acid to produce five different lead-acid batteries with Na contents of 0.02 mol / L, 0.03 mol / L, 0.1 mol / L, 0.3 mol / L and 0.35 mol / L, respectively.

[0130] Furthermore, when the electrode assembly was inserted into the battery case, the height of the ribs provided in the battery case was adjusted to produce five different lead-acid batteries having inter-electrode gaps W of 0.2 mm, 0.15 mm, 0.1 mm, 0 mm, and -0.1 mm, respectively.

[0131] In addition, 25 types of lead acid batteries A2 to A26 with different combinations of interelectrode gap W and Na content in the electrolyte were prepared in the same manner as lead acid battery A1. Table 1 shows the interelectrode gap W and Na content in the electrolyte of lead acid batteries A1 to A26.

[0132] 《Lead-acid battery B1》

[0133] As a separator, a separator having a first rib on the inner side of the bag was used. The separator had a plurality of striped first ribs on the inner side of the bag, and the plurality of first ribs were formed along the height direction of the negative electrode plate, the height of the first rib was 0.1 mm, and the spacing between the first ribs in the region facing the negative electrode plate was 1 mm. The height and spacing of the second ribs and the average thickness of the base portion of the separator were the same as those of the lead-acid battery A1.

[0134] Lead acid battery B1 was assembled in the same manner as lead acid battery A1 except that separators having ribs provided on both sides of the positive electrode plate side and the negative electrode plate side were used.

[0135] 《Lead-acid batteries B2~B26》

[0136] Using the same method as lead acid batteries A2 to A26, 25 types of lead acid batteries with different combinations of interelectrode gap W and Na content in the electrolyte were prepared for lead acid batteries B1 to prepare lead acid batteries B2 to B26. Table 2 shows the interelectrode gap W and Na content in the electrolyte of lead acid batteries B1 to B26.

[0137] [Evaluation 1: Lead sulfate accumulation]

[0138] According to SBAS 0101:2014, the lead-acid battery is charged and discharged under the idling stop condition. Specifically, at 25°C, the following (a) to (c) are regarded as one cycle, and are repeated until the discharge end voltage reaches 1.2V or less per battery cell, and the number of cycles at this time is calculated. It should be noted that during charging and discharging, a rest period of 40 to 48 hours is required every 3600 cycles.

[0139] (a) Discharge 1: Discharge at a current value of 32 A for 59 seconds.

[0140] (b) Discharge 2: Discharge at a current of 300 A for 1 second.

[0141] (c) Charging: Charging for 60 seconds at a limited current of 100 A and a voltage of 2.33 V per battery cell.

[0142] After the charge and discharge test, the end plates are removed from the lead-acid battery and any one negative plate is taken out. After washing and drying, all the electrode materials are taken out and crushed. The sulfur content in the crushed sample is measured using a sulfur analyzer to calculate the lead sulfate accumulation. The lead sulfate accumulation is divided by the number of PSOC life cycles to calculate the lead sulfate accumulation per cycle.

[0143] The above-mentioned lead sulfate storage amount per one cycle was evaluated by expressing it as a relative ratio with the lead sulfate storage amount of the lead storage battery A1 being 100. Tables 1 and 2 show the evaluation results.

[0144] [Evaluation 2: Discharge performance]

[0145] The RC (Reserve Capacity) discharge capacity was measured in accordance with JIS D 5301. The measured discharge capacity was expressed as a relative ratio with the discharge capacity of lead acid battery A1 being 100, and the evaluation was performed. The evaluation results are shown in Tables 1 and 2. A larger evaluation value means a better discharge performance.

[0146] According to Tables 1 and 2, the more the Na content increases, the more the lead sulfate accumulation increases. In addition, there is a trend of reduced discharge capacity. As shown in Table 1, in the lead-acid batteries A2 to A26 where the first rib is not provided on the negative electrode side, the increase in the lead sulfate accumulation can be suppressed by narrowing the inter-electrode gap W and compressing the pole plate group. However, in the lead-acid batteries A2 to A26, the inhibitory effect of lead sulfate accumulation is not sufficient. When the Na content is 0.3 mol / L or more and is contained in a high concentration, it is difficult to reduce the lead sulfate accumulation even if the inter-electrode gap W is controlled compared to the lead-acid battery A1 without adding Na. In addition, by compressing the pole plate group, the discharge capacity is greatly reduced.

[0147] On the other hand, in the lead-acid batteries B2 to B26 provided with the first rib on the negative electrode side, as shown in Table 2, by narrowing the inter-electrode gap W and compressing the electrode group, the increase in the lead sulfate accumulation amount was significantly suppressed, and the electrolyte contained Na, while reducing the lead sulfate accumulation amount to nearly half of that of the lead-acid battery A1. In addition, the reduction in discharge capacity accompanying the compression of the electrode group was also suppressed.

[0148] In addition, the separator after the charge and discharge test was taken out and visually observed for penetration marks. As a result, penetration marks were observed in the lead-acid batteries A1, A2, A7, A12, A17 and A22 in which the Na content was less than 0.02 mol / L and the first rib was not provided on the negative electrode side. On the other hand, in the lead-acid batteries in which the first rib was provided on the negative electrode side, no penetration marks were observed except for the lead-acid battery B1 in which the electrolyte did not contain Na. It is believed that this is because the diffusibility of the electrolyte near the negative plate is improved by providing the first rib on the negative electrode side.

[0149] When the Na content is 0.02 to 0.3 mol / L and the interelectrode gap W is -0.1 to 0.15 mm (lead-acid batteries B7 to B10, B12 to B15, B17 to B20, B22 to B25), the discharge capacity can be maintained at 97% or more based on the lead-acid battery A1, and the accumulation of lead sulfate can be suppressed to 95% or less based on the lead-acid battery A1. At this time, no penetration marks are generated. However, in terms of further suppressing penetration short circuits, the Na content is preferably 0.03 mol / L or more.

[0150] Therefore, lead-acid batteries B8 to B10, B13 to B15, B18 to B20 and B23 to B25 having a Na content of 0.03 to 0.3 mol / L and an interelectrode gap W of -0.1 to 0.15 mm have excellent discharge performance, suppressed accumulation of lead sulfate, and excellent resistance to penetration short circuits.

[0151] [Table 1]

[0152]

[0153] [Agriculture 2]

[0154]

[0155] Industrial Applicability

[0156] The lead acid battery according to one aspect of the present invention can be applied to valve-controlled type and liquid-type lead acid batteries, and can be suitably used as a starting power source for automobiles, motorcycles, and the like.

[0157] Explanation of symbols

[0158] 1: Lead-acid battery

[0159] 2: Negative plate

[0160] 3: Positive plate

[0161] 4: Isolation parts

[0162] 5: Positive electrode shelf

[0163] 6: Negative pole shelf

[0164] 7: Positive column

[0165] 8: Through connector

[0166] 9: Negative column

[0167] 11: Plate group

[0168] 12: Battery tank

[0169] 13: Next Door

[0170] 14: Battery cell room

[0171] 15: Cover

[0172] 16: Negative terminal

[0173] 17: Positive terminal

[0174] 18: Liquid port plug

Claims

1. Lead-acid batteries, with: An electrode plate group including a plurality of positive electrode plates and a plurality of negative electrode plates stacked with separators interposed therebetween, a battery cell chamber for accommodating the electrode assembly, and Electrolyte, The electrolyte contains 0.03 to 0.3 mol / L of Na, The positive electrode plate or the negative electrode plate, i.e., the first end plate, located at one end of the electrode plate group is arranged close to one side of the inner side walls facing each other of the battery cell chamber, and the positive electrode plate or the negative electrode plate, i.e., the second end plate, located at the other end of the electrode plate group is arranged close to the other side of the inner side wall. At this time, the maximum separation distance between the surface of the first end plate facing the inner side wall and the surface of the second end plate facing the inner side wall, i.e., the distance between the end plates, is set to L, the total thickness of the positive electrode plate and the negative electrode plate in the electrode plate group is set to d1, the number of regions where the positive electrode plate and the negative electrode plate face each other in the battery cell chamber, i.e., the number of inter-electrode gaps, is set to N, the total thickness of one of the separators between the positive electrode plate and the negative electrode plate is set to d2, and the inter-electrode gap W calculated by the following formula is -0.1 to +0.15 mm, W={(L-d1) / N}-d2, The separator includes a first rib on the negative electrode plate side.

2. The lead acid battery according to claim 1, wherein The separator includes a second rib on the positive electrode plate side.

3. The lead acid battery according to claim 1 or 2, wherein: The separator is in a bag shape.

4. The lead acid battery according to claim 3, wherein: The separator accommodates the negative electrode plate.

5. The lead acid battery according to claim 3, wherein: The separator accommodates the positive electrode plate.

6. The lead acid battery according to any one of claims 1, 2, 4 and 5, wherein: The negative plate contains a negative electrode material, The negative electrode material contains conductive carbon particles. The carbon particles contain first carbon particles having a particle size of less than 32 μm, The first carbon particles include second carbon particles having a particle diameter smaller than an average pore diameter of the separator.

7. The lead acid battery according to claim 3, wherein: The negative plate contains a negative electrode material, The negative electrode material contains conductive carbon particles. The carbon particles contain first carbon particles having a particle size of less than 32 μm, The first carbon particles include second carbon particles having a particle diameter smaller than an average pore diameter of the separator.

8. The lead acid battery according to claim 6, wherein: The content of the first carbon particles in the negative electrode material is 0.2 mass % to 2 mass %.

9. The lead acid battery according to claim 7, wherein: The content of the first carbon particles in the negative electrode material is 0.2 mass % to 2 mass %.