Cesium fluoride doped all-inorganic perovskite solar cell and preparation method thereof
By doping the perovskite layer with cesium fluoride (CsF), the perovskite layer is optimized, solving the problem of low performance caused by interface defects in inverted all-inorganic perovskite solar cells, improving the energy conversion efficiency and stability of the cells, and making them suitable for commercial production.
Patent Information
- Application Number
- CN202411051315.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
Inverted all-inorganic perovskite solar cells suffer from low performance due to severe nonradiative recombination in the perovskite film, particularly with a large gap between the open-circuit voltage and the theoretical value, which limits the improvement of photoelectric conversion efficiency. This is mainly due to the presence of numerous defects at the interface between the perovskite active layer and the charge collection layer.
By doping the perovskite layer with cesium fluoride (CsF), the perovskite layer is optimized, defects are reduced, and the interface between the electron transport layer and the perovskite layer is passivated. CsF is used as an inorganic metal fluoride additive to control the crystal growth kinetics process, and CsF-doped all-inorganic perovskite solar cells are fabricated.
This method improves the energy conversion efficiency of all-inorganic perovskite solar cells, enhances device stability, and the fabrication process exhibits excellent reproducibility, making it suitable for mass commercial production.
Smart Images

Figure CN118973359A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a cesium fluoride-doped all-inorganic perovskite solar cell and a preparation method thereof. Background Art
[0002] The inverted structure (pin) of all-inorganic perovskite solar cells (PSCs) has attracted widespread attention due to its high light absorption coefficient, excellent carrier transport performance, simple preparation process and high open circuit voltage. In recent years, how to improve the performance of trans all-inorganic solar cells (pin PSCs) has become one of the research hotspots of scientific researchers. At present, the photoelectric energy conversion efficiency of trans all-inorganic perovskite solar cells has reached 21.8%. The perovskite layer plays an indispensable role as a light-absorbing layer. The commonly used perovskite materials are CsPbI 3-x Br x The all-inorganic perovskite itself does not contain organic components. Even when the temperature reaches 350°C, the components and structure can remain stable, and the thermal stability is greatly improved, which is expected to fundamentally solve the decomposition and volatilization of organic components.
[0003] However, due to the perovskite film CsPbI 3-x Br x Severe non-radiative recombination in the device causes the performance of the inverse PSC to be lower than that of traditional perovskite solar cells. Therefore, preparing high-quality perovskite films is one of the keys to improving device performance. For example, the open circuit voltage (Voc) is far from the theoretical value, usually 1.10V (the open circuit voltage of a formal perovskite cell with a similar band gap is greater than 1.20V), resulting in a relatively low photoelectric conversion efficiency of the inverse structure. The main reason is that there are a large number of defects in the perovskite active layer of the device and at the interface between the perovskite active layer and the charge collection layer, which cause non-radiative recombination of photogenerated carriers, resulting in serious energy loss, limiting the improvement of open circuit voltage and photoelectric conversion efficiency.
[0004] Considering the above problems, a new method needs to be developed to optimize the light absorption layer to achieve efficient electron collection, reduce cell defects and improve the energy conversion efficiency of the cell. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the object of the present invention is to provide a cesium fluoride-doped all-inorganic perovskite solar cell and a preparation method thereof, which can optimize the perovskite layer by doping cesium fluoride.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell, comprising the following steps:
[0008] S1: Preparation of PEDOT:PSS hole transport layer on transparent conductive glass;
[0009] S2: Preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x Adding CsF solution into the perovskite precursor solution to prepare a CsF-doped perovskite layer;
[0010] S3: Preparation of PCBM electron transport layer on CsF-doped perovskite layer;
[0011] S4: preparing a BCP buffer layer on the PCBM electron transport layer;
[0012] S5: CsF-doped all-inorganic perovskite solar cells were prepared by depositing silver electrodes on the BCP buffer layer by thermal evaporation.
[0013] In one embodiment, in S1, the process of preparing a PEDOT:PSS hole transport layer on a transparent conductive glass is as follows:
[0014] S11: mixing the PEDOT:PSS stock solution with deionized water to prepare a PEDOT:PSS solution;
[0015] S12: spin coating a PEDOT:PSS solution on the cleaned and ion-bombarded transparent conductive glass, followed by annealing to obtain a PEDOT:PSS hole transport layer;
[0016] In the S11, the volume ratio of the PEDOT:PSS stock solution to deionized water is 1:(1-1.2).
[0017] In one embodiment, in S2, the preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x The process of adding CsF solution to the perovskite precursor solution to prepare the CsF-doped perovskite layer is as follows:
[0018] S21: Dissolve CsI:DMAPbl3:PbBr2 in an anhydrous mixed solvent to prepare CsPbI 3-x Br x Perovskite precursor solution;
[0019] S22: dissolving CsF powder in 1 mL of anhydrous mixed solvent to prepare a CsF solution;
[0020] S23: Towards CsPbI 3-x Br x Adding CsF solution to the perovskite precursor solution to obtain a perovskite solution;
[0021] S24: spin-coating the perovskite solution on the PEDOT:PSS hole transport layer, and then annealing to obtain a CsF-doped perovskite layer.
[0022] In one embodiment, in S21, the molar ratio of CsI:DMAPbl3:PbBr2 is 3:4.85:0.15;
[0023] In S21 and S22, the anhydrous mixed solvent consists of DMF and DMSO, and the volume ratio of DMF to DMSO is 8.5:1.5;
[0024] In S23, the CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution was 4:1.
[0025] In one embodiment, in S22, the concentration of cesium fluoride in the CsF solution is 1.25-10 mg / mL.
[0026] In one embodiment, in S3, the process of preparing a PCBM electron transport layer on the CsF-doped perovskite layer is as follows:
[0027] S31: dissolving PCBM in CB to prepare a PCBM solution;
[0028] S32: spin-coating the PCBM solution on the CsF-doped perovskite layer in a nitrogen environment, and then annealing to obtain a PCBM electron transport layer.
[0029] In one embodiment, in S31, the usage ratio of PCBM to CB is (10-30) mg: 1 mL;
[0030] In the S32, the spin coating amount of the PCBM solution is 40 to 50 uL.
[0031] In one embodiment, in S4, the process of preparing a BCP buffer layer on the PCBM electron transport layer is as follows:
[0032] S41: dissolving BCP in isopropanol to obtain a BCP solution;
[0033] S42: Spin-coat the BCP solution on the PCBM electron transport layer to prepare a BCP buffer layer.
[0034] In one embodiment, in S41, the usage ratio of BCP to isopropanol is (0.5-1) mg:1 mL;
[0035] In the S42, the spin coating amount of the BCP solution is 40 to 50 uL.
[0036] The present invention also provides a cesium fluoride-doped all-inorganic perovskite solar cell prepared by the preparation method, comprising a transparent conductive glass, a PEDOT:PSS hole transport layer, a CsF-doped perovskite layer, a PCBM electron transport layer, a BCP buffer layer and a silver electrode arranged in sequence from bottom to top.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The present invention provides a method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell, which optimizes the perovskite layer by doping cesium fluoride, and improves the energy conversion efficiency of the all-inorganic perovskite solar cell by reducing the defects of the perovskite layer and passivating the interface between the electron transport layer and the perovskite layer. The CsF used as an inorganic metal fluoride additive can control and improve the crystal growth kinetics process, thereby obtaining a well-crystallized perovskite film. Cs ions diffuse into the perovskite film as a passivator, inhibiting ion migration, thereby effectively improving the performance of the PSC. In addition, the method can improve the charge transfer between the electron transport layer and the perovskite interface and reduce charge accumulation, thereby suppressing charge recombination losses to a great extent. The device prepared by the above-mentioned preparation method has improved stability, and the preparation process has excellent repeatability, which is suitable for large-scale commercial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic structural diagram of the inverted perovskite solar cell of the present invention;
[0040] Figure 2 It is a JV curve diagram of the perovskite solar cell prepared from CsF solutions with different concentrations of the present invention. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0042] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0043] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0044] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0045] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0046] The invention provides a cesium fluoride-doped all-inorganic perovskite solar cell and a preparation method thereof.
[0047] On the one hand, a method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell is provided, comprising the following steps:
[0048] S1: Preparation of PEDOT:PSS hole transport layer on transparent conductive glass;
[0049] S2: Preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x Adding CsF solution into the perovskite precursor solution to prepare a CsF-doped perovskite layer;
[0050] S3: Preparation of PCBM electron transport layer on CsF-doped perovskite layer;
[0051] S4: preparing a BCP buffer layer on the PCBM electron transport layer;
[0052] S5: CsF-doped all-inorganic perovskite solar cells were prepared by depositing silver electrodes on the BCP buffer layer by thermal evaporation.
[0053] In one specific embodiment, in S1, the process of preparing a PEDOT:PSS hole transport layer on a transparent conductive glass is as follows:
[0054] S11: mixing the PEDOT:PSS stock solution with deionized water in a volume ratio of 1:(1-1.2) to prepare a PEDOT:PSS solution;
[0055] S12: spin coating a PEDOT:PSS solution on the cleaned and ion-bombarded transparent conductive glass, followed by annealing to obtain a PEDOT:PSS hole transport layer;
[0056] Specifically, in S12, a PEDOT:PSS solution is spin-coated on a transparent conductive glass at a rotation speed of 6000 rpm for 30 seconds; when the PEDOT:PSS hole transport layer is obtained, the annealing temperature is 130° C. and the annealing time is 20 min.
[0057] In one embodiment, in S2, the preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x The process of adding CsF solution to the perovskite precursor solution to prepare the CsF-doped perovskite layer is as follows:
[0058] S21: Dissolve CsI:DMAPbl3:PbBr2 in an anhydrous mixed solvent to prepare CsPbI 3-x Br x Perovskite precursor solution;
[0059] S22: Dissolve 1.25, 2.5 mg, 5 mg, and 10 mg of CsF powder in 1 mL of anhydrous mixed solvent to prepare CsF solutions of different concentrations;
[0060] S23: CsPbI at a volume ratio of 4:1 3-x Br x Adding CsF solution to the perovskite precursor solution to obtain a perovskite solution;
[0061] S24: spin-coating the perovskite solution on the PEDOT:PSS hole transport layer, and then annealing to obtain a CsF-doped perovskite layer.
[0062] Specifically, the molar ratio of CsI:DMAPbl3:PbBr2 is 3:4.85:0.15; the anhydrous mixed solvent consists of DMF and DMSO, and the volume ratio of DMF and DMSO is 8.5:1.5.
[0063] Specifically, the concentration of cesium fluoride in the CsF solution is 1.25 to 10 mg / mL.
[0064] In the S24, the prepared perovskite solution is coated on the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds; when the CsF-doped perovskite layer is obtained, the annealing temperature is 180-200° C. and the annealing time is 3-5 min.
[0065] In a specific embodiment, in S3, the process of preparing the PCBM electron transport layer on the CsF-doped perovskite layer is as follows:
[0066] S31: dissolving PCBM in CB to prepare a PCBM solution;
[0067] S32: spin-coating the PCBM solution on the CsF-doped perovskite layer in a nitrogen environment, and then annealing to obtain a PCBM electron transport layer.
[0068] Specifically, the usage ratio of PCBM to CB is (10-30) mg:1 mL; the spin coating amount of PCBM solution is 40-50 uL.
[0069] In the S32, the PCBM solution is spin-coated on the CsF-doped perovskite layer at a speed of 3000 revolutions for 30 seconds to obtain the PCBM electron transport layer. The annealing temperature is 100° C. (optimum temperature) and the annealing time is 30 minutes.
[0070] In a specific embodiment, in S4, the process of preparing the BCP buffer layer on the PCBM electron transport layer is as follows:
[0071] S41: dissolving BCP in isopropanol to obtain a BCP solution;
[0072] S42: Spin-coat the BCP solution on the PCBM electron transport layer to prepare a BCP buffer layer.
[0073] Specifically, the usage ratio of BCP to isopropanol is (0.5-1) mg:1 mL; the spin coating amount of BCP solution is 40-50 uL.
[0074] In the S42, the BCP solution is spin-coated on the PCBM electron transport layer at a speed of 4000 revolutions per minute for 30 seconds to obtain a BCP buffer layer.
[0075] The cesium fluoride (CsF) used in the present invention is purchased from Aladdin, with a specification of 99.5%, and the storage conditions are: sealed, cool, and dry.
[0076] The PEDOT:PSS stock solution, PCBM, CB and BCP used in the present invention were all purchased from Aladdin.
[0077] In one embodiment, the steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0078] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0079] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0080] In a test tube, mix the PEDOT:PSS stock solution with deionized water in a volume ratio of 1:(1-1.2) and place in an ultrasonic machine for oscillation for 1 h;
[0081] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0082] Step 2: Preparation of CsF-doped perovskite layer:
[0083] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0084] A certain amount (1.25 mg, 2.5 mg, 5 mg, 10 mg) of CsF powder was dissolved in an anhydrous mixed solvent of DMF:DMSO (mixed in a volume ratio of 8.5:1.5), and stirred at room temperature to prepare a CsF solution;
[0085] Add CsF solution to CsPbI according to the quantitative 3-x Br x Perovskite precursor solution (CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution is 4:1), and the perovskite solution is obtained;
[0086] The perovskite film was prepared by spin coating. The prepared perovskite solution was coated on the FTO glass and the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds, and annealed at 180-200°C for 3-5 minutes.
[0087] Step 3: Preparation of PCBM electron transport layer:
[0088] 10-30 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 40-50 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2, and annealed at 100 °C for 30 min.
[0089] Step 4: Preparation of BCP buffer layer:
[0090] Dissolve 0.5-1 mg BCP in 1 mL isopropanol and stir at room temperature;
[0091] Take 40-50uL of the prepared BCP solution and spin-coat it on the electron transport layer PCBM at a speed of 4000 rpm for 30 seconds.
[0092] Step 5: Deposition of silver electrode:
[0093] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0094] like Figure 1 As shown, on the other hand, the present invention provides a cesium fluoride-doped all-inorganic perovskite solar cell prepared by the above-mentioned preparation method, comprising a transparent conductive glass, a PEDOT:PSS hole transport layer, a CsF-doped perovskite layer, a PCBM electron transport layer, a BCP buffer layer and a silver electrode arranged in sequence from bottom to top.
[0095] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0096] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0097] Example 1
[0098] The steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0099] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0100] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0101] In a test tube, the PEDOT:PSS stock solution was mixed with deionized water at a volume ratio of 1:1 and then placed in an ultrasonic machine for oscillation for 1 h;
[0102] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0103] Step 2: Preparation of CsF-doped perovskite layer:
[0104] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0105] 1.25 mg of CsF powder was dissolved in an anhydrous mixed solvent of DMF:DMSO (mixed in a volume ratio of 8.5:1.5) and stirred at room temperature to prepare a CsF solution;
[0106] Add CsF solution to CsPbI according to the quantitative 3-x Br x Perovskite precursor solution (CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution is 4:1), and the perovskite solution is obtained;
[0107] The perovskite film was prepared by spin coating. The prepared perovskite solution was coated on the FTO glass and the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds and annealed at 180°C for 3 minutes.
[0108] Step 3: Preparation of PCBM electron transport layer:
[0109] 10 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 40 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2 and annealed at 100 °C for 30 min.
[0110] Step 4: Preparation of BCP buffer layer:
[0111] Dissolve 0.5 mg of BCP in 1 mL of isopropanol and stir at room temperature;
[0112] Take 40uL of the prepared BCP solution and spin coat it on the electron transport layer PCBM at 4000 rpm for 30 seconds.
[0113] Step 5: Deposition of silver electrode:
[0114] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0115] Example 2
[0116] The steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0117] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0118] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0119] In a test tube, the PEDOT:PSS stock solution was mixed with deionized water at a volume ratio of 1:1.1 and then placed in an ultrasonic machine for oscillation for 1 h;
[0120] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0121] Step 2: Preparation of CsF-doped perovskite layer:
[0122] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0123] A certain amount of 2.5 mg of CsF powder was dissolved in an anhydrous mixed solvent of DMF:DMSO (mixed in a volume ratio of 8.5:1.5) and stirred at room temperature to prepare a CsF solution;
[0124] Add CsF solution to CsPbI according to the quantitative 3-x Br x Perovskite precursor solution (CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution is 4:1), and the perovskite solution is obtained;
[0125] The perovskite film was prepared by spin coating. The prepared perovskite solution was coated on the FTO glass and the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds and annealed at 190°C for 4 minutes.
[0126] Step 3: Preparation of PCBM electron transport layer:
[0127] 20 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 45 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2 and annealed at 100 °C for 30 min.
[0128] Step 4: Preparation of BCP buffer layer:
[0129] Dissolve 0.75 mg of BCP in 1 mL of isopropanol and stir at room temperature;
[0130] Take 45uL of the prepared BCP solution and spin-coat it on the electron transport layer PCBM at a speed of 4000 rpm for 30 seconds.
[0131] Step 5: Deposition of silver electrode:
[0132] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0133] Example 3
[0134] The steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0135] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0136] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0137] In a test tube, the PEDOT:PSS stock solution was mixed with deionized water at a volume ratio of 1:1.2 and then placed in an ultrasonic machine for oscillation for 1 h;
[0138] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0139] Step 2: Preparation of CsF-doped perovskite layer:
[0140] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0141] A certain amount of 5 mg of CsF powder was dissolved in an anhydrous mixed solvent of DMF:DMSO (mixed in a volume ratio of 8.5:1.5) and stirred at room temperature to prepare a CsF solution;
[0142] Add CsF solution to CsPbI according to the quantitative 3-x Br x Perovskite precursor solution (CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution is 4:1), and the perovskite solution is obtained;
[0143] The perovskite film was prepared by spin coating. The prepared perovskite solution was coated on the FTO glass and the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds and annealed at 200°C for 5 minutes.
[0144] Step 3: Preparation of PCBM electron transport layer:
[0145] 30 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 50 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2 and annealed at 100 °C for 30 min.
[0146] Step 4: Preparation of BCP buffer layer:
[0147] Dissolve 1 mg of BCP in 1 mL of isopropanol and stir at room temperature;
[0148] Take 50uL of the prepared BCP solution and spin coat it on the electron transport layer PCBM at 4000 rpm for 30 seconds.
[0149] Step 5: Deposition of silver electrode:
[0150] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0151] Example 4
[0152] The steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0153] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0154] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0155] In a test tube, the PEDOT:PSS stock solution was mixed with deionized water at a volume ratio of 1:1 and then placed in an ultrasonic machine for oscillation for 1 h;
[0156] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0157] Step 2: Preparation of CsF-doped perovskite layer:
[0158] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0159] A certain amount of 10 mg of CsF powder was dissolved in an anhydrous mixed solvent of DMF:DMSO (mixed in a volume ratio of 8.5:1.5) and stirred at room temperature to prepare a CsF solution;
[0160] Add CsF solution to CsPbI according to the quantitative 3-x Br x Perovskite precursor solution (CsPbI 3-x Br xThe volume ratio of the perovskite precursor solution to the CsF solution is 4:1), and the perovskite solution is obtained;
[0161] The perovskite film was prepared by spin coating. The prepared perovskite solution was coated on the FTO glass and the PEDOT:PSS hole transport layer at a speed of 4500 rpm for 30 seconds and annealed at 200°C for 4 minutes.
[0162] Step 3: Preparation of PCBM electron transport layer:
[0163] 20 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 40 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2 and annealed at 100 °C for 30 min.
[0164] Step 4: Preparation of BCP buffer layer:
[0165] Dissolve 0.5 mg of BCP in 1 mL of isopropanol and stir at room temperature;
[0166] Take 40uL of the prepared BCP solution and spin coat it on the electron transport layer PCBM at 4000 rpm for 30 seconds.
[0167] Step 5: Deposition of silver electrode:
[0168] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0169] Comparative Example
[0170] The steps of the preparation method of cesium fluoride doped all-inorganic perovskite solar cell are as follows:
[0171] Step 1: Preparation of PEDOT:PSS hole transport layer:
[0172] FTO transparent conductive glass (2.47 cm × 2.47 cm) was ultrasonically cleaned with deionized water, isopropanol, acetone, and ethanol for 30 min in sequence. The FTO glass was removed from the anhydrous alcohol and dried with nitrogen gas.
[0173] In a test tube, the PEDOT:PSS stock solution was mixed with deionized water at a volume ratio of 1:1.1 and then placed in an ultrasonic machine for oscillation for 1 h;
[0174] After the cleaned FTO glass was subjected to ion bombardment treatment to further remove moisture and impurities on the glass surface, the prepared PEDOT:PSS solution was spin-coated on the FTO glass at a speed of 6000 rpm for 30 seconds and annealed at 130°C for 20 minutes.
[0175] Step 2: Preparation of perovskite layer:
[0176] The concentration of the perovskite solution was maintained at 0.6 M, and CsI:DMAPbl3:PbBr2 was dissolved in an anhydrous mixed solvent DMF:DMSO (mixed in a volume ratio of 8.5:1.5) at a molar ratio of 3:4.85:0.15 to prepare CsPbI 3-x Br x Perovskite precursor solution; the perovskite precursor solution was stirred at room temperature for 2 h and filtered through a 0.2 uL syringe filter;
[0177] The perovskite film was prepared by spin coating. The prepared CsPbI 3-x Br x The perovskite precursor solution was coated on FTO glass and PEDOT:PSS hole transport layer and annealed at 190 °C for 4 min.
[0178] Step 3: Preparation of PCBM electron transport layer:
[0179] 20 mg of PCBM was dissolved in 1 mL of CB and stirred at room temperature. 45 uL of PCBM solution was spin-coated on the perovskite layer at 3000 rpm for 30 seconds in a glove box filled with N2 and annealed at 100 °C for 30 min.
[0180] Step 4: Preparation of BCP buffer layer:
[0181] Dissolve 0.75 mg of BCP in 1 mL of isopropanol and stir at room temperature;
[0182] Take 45uL of the prepared BCP solution and spin-coat it on the electron transport layer PCBM at a speed of 4000 rpm for 30 seconds.
[0183] Step 5: Deposition of silver electrode:
[0184] A perovskite solar cell device was fabricated by depositing about 70 nm thick Ag on top by thermal evaporation.
[0185] Table 1 Main performance parameters of perovskite solar cells at different CsF concentrations
[0186]
[0187] The main performance parameters of perovskite solar cells under different cesium fluoride concentrations are shown in Table 1. When the cesium fluoride concentration is 2.5 mg / mL, the open circuit voltage of the device is 0.99 V and the short circuit current is 17.38 mA / cm 2 , the filling factor is 61.82, the photoelectric conversion efficiency is 12.63%, and the JV curve is as follows Figure 2 shown.
[0188] As the concentration of cesium fluoride increases, the efficiency of perovskite solar cells increases until 2.5 mg / mL, when the photoelectric conversion efficiency is the highest. When the concentration reaches 5 mg / mL, the efficiency begins to decrease.
[0189] The present invention significantly improves the open circuit voltage, short circuit current density, fill factor and photoelectric conversion efficiency of the all-inorganic perovskite solar cell by trying additives of different concentrations.
[0190] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell, characterized in that: The following steps are involved: S1: Preparation of PEDOT:PSS hole transport layer on transparent conductive glass; S2: Preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x Adding CsF solution into the perovskite precursor solution to prepare a CsF-doped perovskite layer; S3: Preparation of PCBM electron transport layer on CsF-doped perovskite layer; S4: preparing a BCP buffer layer on the PCBM electron transport layer; S5: CsF-doped all-inorganic perovskite solar cells were prepared by depositing silver electrodes on the BCP buffer layer by thermal evaporation.
2. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 1, characterized in that: In S1, the process of preparing the PEDOT:PSS hole transport layer on the transparent conductive glass is as follows: S11: mixing the PEDOT:PSS stock solution with deionized water to prepare a PEDOT:PSS solution; S12: spin coating a PEDOT:PSS solution on the cleaned and ion-bombarded transparent conductive glass, followed by annealing to obtain a PEDOT:PSS hole transport layer; In the S11, the volume ratio of the PEDOT:PSS stock solution to deionized water is 1:(1-1.2).
3. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 1, characterized in that: In S2, the preparation of CsPbI 3-x Br x Perovskite precursor solution, preparation of CsF solution, to CsPbI 3-x Br x The process of adding CsF solution to the perovskite precursor solution to prepare the CsF-doped perovskite layer is as follows: S21: Dissolve CsI:DMAPbl3:PbBr2 in an anhydrous mixed solvent to prepare CsPbI 3-x Br x Perovskite precursor solution; S22: dissolving CsF powder in 1 mL of anhydrous mixed solvent to prepare a CsF solution; S23: Towards CsPbI 3-x Br x Adding CsF solution to the perovskite precursor solution to obtain a perovskite solution; S24: spin-coating the perovskite solution on the PEDOT:PSS hole transport layer, and then annealing to obtain a CsF-doped perovskite layer.
4. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 3, characterized in that: In S21, the molar ratio of CsI:DMAPbl3:PbBr2 is 3:4.85:0.15; In S21 and S22, the anhydrous mixed solvent consists of DMF and DMSO, and the volume ratio of DMF to DMSO is 8.5:1.5; In S23, the CsPbI 3-x Br x The volume ratio of the perovskite precursor solution to the CsF solution was 4:
1.
5. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 3, characterized in that: In the S22, the concentration of cesium fluoride in the CsF solution is 1.25-10 mg / mL.
6. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 1, characterized in that: In S3, the process of preparing the PCBM electron transport layer on the CsF-doped perovskite layer is as follows: S31: dissolving PCBM in CB to prepare a PCBM solution; S32: spin-coating the PCBM solution on the CsF-doped perovskite layer in a nitrogen environment, and then annealing to obtain a PCBM electron transport layer.
7. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 6, characterized in that: In S31, the dosage ratio of PCBM to CB is (10-30) mg: 1 mL; In the S32, the spin coating amount of the PCBM solution is 40 to 50 uL.
8. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 1, characterized in that: In S4, the process of preparing the BCP buffer layer on the PCBM electron transport layer is as follows: S41: dissolving BCP in isopropanol to obtain a BCP solution; S42: Spin-coat the BCP solution on the PCBM electron transport layer to prepare a BCP buffer layer.
9. The method for preparing a cesium fluoride-doped all-inorganic perovskite solar cell according to claim 8, characterized in that: In S41, the dosage ratio of BCP to isopropanol is (0.5-1) mg:1 mL; In the S42, the spin coating amount of the BCP solution is 40 to 50 uL.
10. A cesium fluoride-doped all-inorganic perovskite solar cell prepared according to the preparation method according to any one of claims 1 to 9, characterized in that: It includes transparent conductive glass, a PEDOT:PSS hole transport layer, a CsF-doped perovskite layer, a PCBM electron transport layer, a BCP buffer layer and a silver electrode, which are arranged in sequence from bottom to top.
Citation Information
Cited By
Method for improving performance of perovskite material
CN119384201A
A method for improving the performance of perovskite materials
CN119384201B
Preparation method of novel perovskite light-emitting diode
CN119562740A
High-purity villiaumite slurry, preparation method and application
CN122609093A
High-purity fluorine salt slurry, preparation method and application
CN122609093B