Processing tank for manufacturing polarizing film and manufacturing device for polarizing film
By using a high-elongation coating and a stainless steel tank body in the processing tank of the polarizing film manufacturing device, the problem of processing liquid erosion is solved, the frequency of maintenance is reduced, and the service life of the equipment is extended.
Patent Information
- Application Number
- CN201911265458.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-12
- Filing Date
- 2019-12-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-12-11
AI Technical Summary
After long-term use of the treatment tank of the existing polarizing film manufacturing device, due to cracks or peeling of the coating layer, the treatment liquid corrodes the main body of the tank, which requires repair or replacement, and the maintenance frequency is high.
A coating layer formed of a coating material with an elongation of more than 150%, combined with an appropriate thermal expansion coefficient and thickness, is covered on the metal tank body to ensure that the treatment liquid does not come into contact with the tank body, and stainless steel materials are used in the tank body to reduce erosion risk.
It effectively prevents the treatment liquid from corroding the main body of the tank, reduces the frequency of maintenance, extends the service life of the treatment tank, and ensures the continuity of the polarizing film manufacturing process.
Smart Images

Figure CN111308601B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a treatment tank used when a polarizing film is manufactured by immersing an original film roll in a treatment liquid and a manufacturing device for the polarizing film. Background Art
[0002] Polarizing films have been conventionally used as constituent materials for liquid crystal display devices, polarized sunglasses, etc. As the polarizing films, for example, films dyed with a dichroic substance such as iodine are known.
[0003] Such a polarizing film is obtained, for example, by immersing a polyvinyl alcohol-based film as an original film roll in a swelling treatment tank, a dyeing treatment tank, a crosslinking treatment tank, a stretching treatment tank, and a washing treatment tank in this order (Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2013-210520 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, each treatment tank such as the cross-linking treatment tank contains each treatment liquid such as a cross-linking treatment liquid. The treatment tank is composed of a metal tank body and a coating layer covering the inner surface of the tank body. The coating layer is used to prevent the metal tank body from being corroded by the treatment liquid such as the cross-linking treatment liquid, and is formed of FRP (fiber reinforced composite material) such as fiber reinforced epoxy resin.
[0009] However, during long-term use, the coating may crack or peel off from the tank body. Once the coating cracks or peels off, the treatment liquid will contact the tank body from that part, so the tank body will be corroded by the treatment liquid, and the treatment tank has to be repaired / replaced.
[0010] An object of the present invention is to provide a processing tank for producing a polarizing film and a manufacturing apparatus for the polarizing film which are not easily corroded by a processing liquid contained therein.
[0011] Solutions for solving problems
[0012] Regarding the processing tank for manufacturing polarizing film of the present invention, in the processing tank for containing the processing liquid used when making polarizing film from the film original roll, the above-mentioned processing tank has a metal tank body and a coating layer covering the inner surface of the above-mentioned tank body, and the above-mentioned coating layer is formed by a coating material with an elongation of more than 150%.
[0013] In a preferred treatment tank for producing a polarizing film of the present invention, the coating layer is formed of a coating material having an elongation of 350% to 450%.
[0014] In the preferred processing tank for producing polarizing film of the present invention, the thermal expansion coefficient of the tank body is 10×10 -6 / ℃~24×10 -6 / ℃.
[0015] In the preferred treatment tank for producing a polarizing film of the present invention, the covering material contains a polyurea resin.
[0016] In the preferred treatment tank for producing a polarizing film of the present invention, the coating layer has a thickness of 1.0 mm or more.
[0017] In the preferred processing tank for producing a polarizing film of the present invention, the tank body is formed of stainless steel.
[0018] The treatment tank for producing a polarizing film of the present invention is preferably used for at least one of a cross-linking treatment tank for cross-linking an original film roll and a stretching treatment tank for stretching an original film roll.
[0019] According to another aspect of the present invention, a device for manufacturing a polarizing film is provided.
[0020] The manufacturing apparatus for manufacturing a polarizing film of the present invention comprises any of the above-mentioned treatment tanks, a treatment liquid contained in the treatment tank, and a conveying device for conveying a film original roll and immersing the film original roll in the treatment liquid in the treatment tank.
[0021] In a preferred polarizing film manufacturing apparatus of the present invention, the treatment liquid contains at least one of an iodine compound and a boron compound.
[0022] In a preferred polarizing film manufacturing apparatus of the present invention, the temperature of the processing liquid is 40° C. or higher.
[0023] Effects of the Invention
[0024] The treatment tank for producing polarizing films of the present invention is not easily corroded by the treatment liquid and can be used for producing polarizing films for a long time without repair or replacement.
[0025] Furthermore, the manufacturing device having the aforementioned processing tank can reduce the maintenance frequency of the processing tank and can manufacture polarizing films for a long period of time. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a cross-sectional view of a treatment tank for producing a polarizing film according to one embodiment of the present invention.
[0027] Figure 2It is a schematic diagram showing the manufacturing apparatus of the polarizing film of this invention.
[0028] Description of Reference Numerals
[0029] 1 Processing tank
[0030] 1A Swelling treatment tank
[0031] 1B Dyeing treatment tank
[0032] 1C Cross-linking treatment tank
[0033] 1D stretch processing tank
[0034] 1E Washing tank
[0035] 11 slot body
[0036] 12 Coating layer
[0037] 2. Polarizing film manufacturing device
[0038] 3 Film roll DETAILED DESCRIPTION
[0039] In this specification, the numerical range expressed as "lower limit value X to upper limit value Y" means greater than or equal to the lower limit value X and less than or equal to the upper limit value Y. When a plurality of numerical ranges are described, "arbitrary lower limit value to arbitrary upper limit value" can be set by selecting any lower limit value and any upper limit value.
[0040] The drawings are provided for reference only, and it should be noted that the sizes, scales, and shapes of components and the like shown in the drawings may be different from the actual ones.
[0041] The treatment tank for producing a polarizing film of the present invention is a container for containing a treatment liquid used when producing a polarizing film from an original film roll.
[0042] As a method for manufacturing a polarizing film from a film stock roll, for example, there are steps of swelling the film stock roll with a swelling treatment liquid, dyeing the swollen film stock roll with a dyeing treatment liquid, and cross-linking the dyed film stock roll with a cross-linking treatment liquid, and preferably also a step of washing the film stock roll with a washing treatment liquid. In addition, the above-mentioned manufacturing method also has: a step of stretching the film stock roll in a stretching treatment liquid after the above-mentioned cross-linking step, or a step of stretching the film stock roll in at least one step selected from the above-mentioned swelling step, dyeing step and cross-linking step, or a step of stretching the film stock roll in at least one step selected from the above-mentioned swelling step, dyeing step and cross-linking step and stretching the film stock roll in a stretching treatment liquid after the cross-linking step.
[0043] The treatment tank of the present invention is installed in a production line of polarizing films in a state where the treatment liquid such as the swelling treatment liquid is contained.
[0044] [Processing tank for polarizing film production]
[0045] Figure 1 It is a cross-sectional view of a processing tank 1 for producing a polarizing film.
[0046] Reference Figure 1 The treatment tank 1 comprises a tank body 11 made of metal and a coating layer 12 covering the inner surface of the tank body 11. In the present invention, the coating layer 12 is formed of a coating material having an elongation of 150% or more.
[0047] Specifically, the shape of the tank body 11 is not particularly limited as long as it can accommodate the processing liquid inside and has an entrance and exit for carrying in and out the original film roll. In the example shown in the figure, the tank body 11 is formed into a concave shape with an upper surface opening, having a bottom portion 111 and a peripheral wall portion 112 rising from the periphery of the bottom portion 111. In the tank body 11 with an upper surface opening, the upper surface opening becomes the entrance and exit of the original film roll. It should be noted that the cover material (not shown) formed with the entrance and exit of the original film roll can cover the upper surface opening of the aforementioned tank body 11. In addition, the entrance and exit of the original film roll can be formed in the upper part of the peripheral wall portion 112 of the tank body 11 (not shown).
[0048] The thermal expansion coefficient of the tank body 11 is preferably 10×10 -6 / ℃~24×10 -6 / °C, and more preferably 10×10 -6 / ℃~18×10 -6 / °C, more preferably 15×10 -6 / ℃~18×10 -6 By providing the coating layer 12 having an elongation of 150% or more to the tank body 11 having a thermal expansion coefficient in the above range, cracking or peeling of the coating layer 12 can be prevented even when the processing tank 1 is used for a long period of time.
[0049] The thermal expansion coefficient is a value representing a change in length or volume of an object due to a temperature rise as a rate of change per 1°C.
[0050] The thermal expansion coefficient of the groove body 11 is the thermal expansion coefficient of the groove body 11 itself without the coating layer 12 etc. Usually, the thermal expansion coefficient of the groove body 11 is equal to the thermal expansion coefficient of the metal forming the groove body 11.
[0051] In addition, the said thermal expansion coefficient is an average value in 0 degreeC - 100 degreeC. The said thermal expansion coefficient is measured according to JIS Z2285:2003 (the measurement method of the linear thermal expansion coefficient of a metal material).
[0052] The metal forming the groove body 11 is not particularly limited, but preferably, a metal having the aforementioned 10×10 -6 / ℃~24×10 -6 / ℃ thermal expansion coefficient of metal. For example, as the metal forming the tank body 11, stainless steel, iron, aluminum, alloys, etc. can be listed, and stainless steel is preferably used. Stainless steel is specified in the JIS standard as various materials such as SUS304, SUS305, SUS316, SUS410, SUS430, etc. The present invention can appropriately select and use from these stainless steels, preferably using SUS316L or SUS304. It should be noted that the thermal expansion coefficient of SUS304 is 17.3×10 -6 / ℃, the thermal expansion coefficient of SUS316L is 16.0×10 -6 / ℃.
[0053] The thickness of the tank body 11 is not particularly limited as long as it has a mechanical strength sufficient to accommodate the treatment liquid. If the thickness is too large, the material cost will increase. From this perspective, the thickness of the tank body 11 is, for example, 0.5 mm to 10 mm, preferably 2 mm to 6 mm, and more preferably 2.5 mm to 5 mm.
[0054] The coating layer 12 is a coating provided on the inner surface of the tank body 11 in order to prevent the processing liquid from coming into contact with the inner surface of the tank body 11 .
[0055] In the example shown in the figure, the coating layer 12 is continuously provided without a gap from the inner surface of the bottom surface portion 111 of the tank body 11 to the inner surface of the peripheral wall surface portion 112 .
[0056] It should be noted that, in the example shown in the figure, the coating layer 12 is provided without gaps on the entire inner surface of the tank body 11, but there may be a portion of the inner surface of the tank body 11 where the coating layer 12 is not provided. As described above, the coating layer 12 is provided to prevent the processing liquid from contacting the tank body 11, so the coating layer 12 may not be provided at a portion of the inner surface of the tank body 11 where the processing liquid obviously does not contact. Examples of the portion where the processing liquid obviously does not contact include the upper end of the peripheral wall surface 112 on the inner surface of the tank body 11.
[0057] The coating layer 12 is formed of a coating material having an elongation of 150% or more. Preferably, the coating layer 12 is formed of a coating material having an elongation of 350% or more, and more preferably, a coating material having an elongation of 375% or more. There is no upper limit to the elongation of the material forming the coating layer 12, but, for example, the elongation of the coating material is 500% or less, preferably 450% or less.
[0058] Here, the elongation is determined by measuring the length before stretching and the length at break in a tensile test and then calculating elongation (%) = (length at break - length before stretching) / length before stretching.
[0059] The specific method for measuring the elongation of the covering material can be measured by a tensile test in accordance with ASTM-D412 under standard conditions (23° C., 1 atmosphere, 50% RH).
[0060] In addition, the material forming the coating layer 12 may be a material that is not easily corroded by the treatment liquid. Hereinafter, the property of not being easily corroded by the treatment liquid is referred to as corrosion resistance. In particular, the coating material preferably has corrosion resistance to a treatment liquid containing at least one of an iodine compound such as potassium iodide and sodium iodide and a boron compound, and more preferably has corrosion resistance to a treatment liquid containing at least one of potassium iodide and boric acid.
[0061] The coating material is not particularly limited as long as it has an elongation of 150% or more and has corrosion resistance. Specifically, examples of the coating material include polyurea resin, rubber, and elastomer, and a material containing polyurea resin is particularly preferred.
[0062] The polyurea resin is a resin having a urea bond formed by a chemical reaction between an isocyanate group and an amino group. Examples of the polyurea resin include polymers obtained by reacting polyisocyanates with polyamines.
[0063] There is no particular limitation on the method of forming the coating layer 12 on the inner surface of the tank body 11, and a suitable method can be appropriately adopted according to the coating material. For example, in the case of using polyurea resin as the coating material, the coating layer 12 can be formed by spraying the polyurea resin onto the tank body 11 using a coating machine. In addition, without being limited to a coating machine, the polyurea resin can also be applied to the tank body 11 by hand. Regarding two-component polyurea resins, it is possible to apply them while allowing the two components (isocyanate and amine) to react. As mentioned above, the polyurea resin can be applied by spraying or hand coating. Therefore, even if cracks or peeling occur in the coating layer, there is no need to replace the processing tank, and the polyurea resin can be locally applied or overcoated at the location where the cracks occur, so that the processing tank can be easily repaired.
[0064] The thickness of the coating layer 12 is not particularly limited. If it is too small, the coating layer 12 will follow the deformation of the tank body 11 and stretch, so there is a risk that the thickness of the coating layer 12 is partially too small. From this point of view, the thickness of the coating layer 12 is preferably 1 mm or more, more preferably 1.5 mm or more, and further preferably 2 mm or more. In addition, there is no upper limit to the thickness of the coating layer 12, but in consideration of cost effectiveness, it is 10 mm or less, preferably 4 mm or less.
[0065] Hereinafter, the treatment tank 1 described in the section [Treatment tank for producing polarizing film] may be referred to as “specific treatment tank 1 ”.
[0066] [Polarizing film manufacturing device]
[0067] The manufacturing device of the polarizing film of the present invention is a device for carrying out the following steps: performing a predetermined treatment of immersing a film stock roll in a treatment tank containing a treatment liquid to obtain a polarizing film from the film stock roll. That is, the film stock roll subjected to the predetermined treatment by the manufacturing device is a polarizing film.
[0068] The polarizing film manufacturing device of the present invention comprises one or more treatment tanks for containing treatment liquid for treating the film original roll, the treatment liquid contained in the aforementioned treatment tank, and a conveying device for conveying the film original roll and immersing it in the treatment liquid in the aforementioned treatment tank.
[0069] As at least one of the processing tanks of the production apparatus, the above-mentioned specific processing tank 1 can be used.
[0070] Figure 2 1 is a reference diagram showing a polarizing film manufacturing apparatus 2. The arrow in the figure indicates the moving direction (conveying direction) of the original film roll 3.
[0071] The manufacturing apparatus 2 includes a front roll unit 28 around which the original film roll 3 to be processed is wound, and a rear roll unit 29 for winding up the polarizing film. The manufacturing apparatus 2 manufactures the polarizing film by a so-called roll-to-roll method.
[0072] Various treatment tanks are arranged between the front roller section 28 and the rear roller section 29. Examples of the treatment tanks include a swelling treatment tank containing a swelling treatment liquid, a dyeing treatment tank containing a dyeing treatment liquid, a cross-linking treatment tank containing a cross-linking treatment liquid, a stretching treatment tank containing a stretching treatment liquid, and a washing treatment tank containing a washing treatment liquid.
[0073] The manufacturing apparatus 2 shown in the figure includes a swelling treatment tank 1A, a dyeing treatment tank 1B, a cross-linking treatment tank 1C, a stretching treatment tank 1D, and a washing treatment tank 1E in this order from the front roll section 28 to the rear roll section 29 .
[0074] The specific treatment tank 1 is used for at least one selected from the swelling treatment tank 1A, dyeing treatment tank 1B, cross-linking treatment tank 1C, stretching treatment tank 1D and washing treatment tank 1E, preferably for two or more. It should be noted that the specific treatment tank 1 can also be used for all treatment tanks contained in the manufacturing device 2.
[0075] The specific treatment tank 1 is preferably a treatment tank for containing at least one of an iodine compound and a boron compound. Iodine compounds such as potassium iodide and boron compounds such as boric acid easily corrode the metal tank body 11. Therefore, by using the specific treatment tank 1, even when such a treatment liquid is contained, the corrosion of the tank body 11 can be effectively prevented.
[0076] As treatment tanks for containing a treatment liquid containing at least one of potassium iodide (iodine compound) and boric acid (boron compound), there can be listed swelling treatment tank 1A, dyeing treatment tank 1B, cross-linking treatment tank 1C, stretching treatment tank 1D and adjustment treatment tank, as described later.
[0077] From the viewpoint of the components of the treatment liquid, the specific treatment tank 1 is preferably used for at least the stretching treatment tank 1D, and further, more preferably used for at least the cross-linking treatment tank 1C and the stretching treatment tank 1D. For example, from the viewpoint of the components of the treatment liquid, the specific treatment tank 1 can be used for the swelling treatment tank 1A, the dyeing treatment tank 1B, the cross-linking treatment tank 1C, the stretching treatment tank 1D, and the adjustment treatment tank.
[0078] In addition, the specific treatment tank 1 is preferably a treatment tank for containing at least a treatment liquid having a temperature of 40°C or more (preferably 60°C or more). When the temperature of the treatment liquid is high, the metal tank body 11 undergoes thermal expansion, and there is a risk of cracking or partial peeling of the coating layer 12. The coating layer 12 of the specific treatment tank 1 follows the thermal expansion of the tank body 11, so even when such a treatment liquid is contained, cracking or peeling of the coating layer 12 can be effectively prevented.
[0079] When producing a polarizing film, examples of the treatment liquid for adjusting the liquid temperature to 40° C. or higher include a dyeing treatment liquid, a crosslinking treatment liquid, and a stretching treatment liquid, as described below.
[0080] From the viewpoint of the temperature of the treatment liquid, the specific treatment tank 1 is preferably used at least in the stretching treatment tank 1D, and further, more preferably at least in the cross-linking treatment tank 1C and the stretching treatment tank 1D. For example, from the viewpoint of the temperature of the treatment liquid, the specific treatment tank 1 can be used in the dyeing treatment tank 1B, the cross-linking treatment tank 1C, and the stretching treatment tank 1D, respectively.
[0081] In the example shown in the figure, the crosslinking treatment tank 1C and the stretching treatment tank 1D are both constituted by the specific treatment tank 1, and the swelling treatment tank 1A, the dyeing treatment tank 1B and the washing treatment tank 1E are all constituted by treatment tanks other than the specific treatment tank. However, this is only an example, and the specific treatment tank 1 can be used in an appropriate part.
[0082] Furthermore, in order to convey the original film roll 3 from the front roller unit 28 to the rear roller unit 29 through the processing tank, a conveying device for the original film roll 3 is provided between the front roller unit 28 and the rear roller unit 29 .
[0083] The conveying device includes a plurality of nip rollers 24 , a plurality of guide rollers 25 , and a driving device (a motor or the like, not shown) for driving at least one roller selected from the nip rollers 24 and the guide rollers 25 to convey the original film roll 3 .
[0084] A plurality of guide rollers 25 are disposed in each treatment tank. The original film roll 3 passes through the nip rollers 24 and the guide rollers 25 and is transported from the front roller section 28 to the rear roller section 29 while being immersed in the treatment liquid in each treatment tank.
[0085] <Original film roll>
[0086] The original film roll 3 before being processed is wound around the front roller unit 28 .
[0087] The aforementioned film original roll 3 is in the shape of a strip. The strip refers to a rectangular shape whose length in the longitudinal direction is sufficiently greater than the length in the width direction (a direction perpendicular to the longitudinal direction). The length in the longitudinal direction of the strip-shaped film original roll 3 is, for example, 10 m or more, preferably 50 m or more.
[0088] The film original roll 3 is not particularly limited. Due to the excellent dyeability based on the dichroic substance, it is preferred to use a film including a hydrophilic polymer film (such as a polyvinyl alcohol-based film, etc.), and more preferably a hydrophilic polymer film. As the aforementioned film including a hydrophilic polymer film, a film formed by laminating a hydrophilic polymer film and a non-hydrophilic polymer film can be listed. In this case, it is preferred that the aforementioned hydrophilic polymer film is laminated on the surface and / or back of the non-hydrophilic polymer film. In this case, the hydrophilic polymer film laminated on the surface and / or back of the non-hydrophilic polymer film can be a thin film with a thickness of about several μm.
[0089] As the aforementioned hydrophilic polymer film, there is no particular limitation, and existing known films can be used. Specifically, as the hydrophilic polymer film, for example, polyvinyl alcohol (PVA) films, partially formalized PVA films, polyethylene terephthalate (PET) films, ethylene-vinyl acetate copolymer films, and partially saponified films thereof can be cited. In addition, in addition to these, polyene oriented films such as dehydrated PVA, dehydrochlorinated polyvinyl chloride, and stretched oriented polyvinylidene films can also be used. Among these, due to the excellent dyeability based on dichroic substances, PVA polymer films are particularly preferred.
[0090] Examples of the raw material polymer of the PVA polymer film include polymers obtained by polymerizing vinyl acetate and then saponifying it, polymers obtained by copolymerizing vinyl acetate with a small amount of copolymerizable monomers such as unsaturated carboxylic acid and unsaturated sulfonic acid, etc. The degree of polymerization of the PVA polymer is not particularly limited, but is preferably 500 to 10,000, more preferably 1,000 to 6,000, from the perspective of solubility in water. In addition, the degree of saponification of the PVA polymer is preferably 75 mol% or more, more preferably 98 mol% to 100 mol%.
[0091] The thickness of the original film roll 3 before treatment is not particularly limited, and is, for example, 15 μm to 110 μm. It should be noted that the original film roll 3 before treatment having a thickness of 38 μm to 110 μm or 50 μm to 100 μm can be used.
[0092] <Swelling treatment tank>
[0093] The swelling treatment tank 1A is a treatment tank that contains a swelling treatment liquid 41. The swelling treatment tank 1A causes the original film roll 3 to swell.
[0094] In addition, although only one swelling treatment tank 1A is provided in the example of the figure, two or more swelling treatment tanks 1A may be arranged in a row in the moving direction of the original film roll 3 (not shown).
[0095] The swelling treatment liquid 41 charged into the swelling treatment tank 1A is a treatment liquid for swelling the original film roll 3 before treatment.
[0096] As the swelling treatment liquid 41, water can be used, for example. Furthermore, water prepared by adding an appropriate amount of an iodine compound such as glycerol or potassium iodide to water can be used as the swelling treatment liquid. When glycerol is added, the concentration is preferably 5% by weight or less, and when an iodine compound such as potassium iodide is added, the concentration is preferably 10% by weight or less.
[0097] <Dyeing treatment tank>
[0098] The dyeing treatment tank 1B is a treatment tank that contains a dyeing treatment liquid 42. The dyeing treatment tank 1B dyes the original film roll 3.
[0099] In addition, although only one dyeing treatment tank 1B is provided in the example of the figure, two or more dyeing treatment tanks 1B may be arranged in a row in the moving direction of the original film roll 3 (not shown).
[0100] The dyeing treatment liquid 42 is a treatment liquid for dyeing the original film roll 3 .
[0101] The dyeing treatment liquid 42 may be a solution containing a dichroic substance as an effective component. Examples of the dichroic substance include iodine and organic dyes.
[0102] Preferably, as the dyeing treatment liquid 42, a solution obtained by dissolving iodine in a solvent can be used. As the solvent, water is generally used, but an organic solvent compatible with water can be further added. The concentration of iodine in the dyeing treatment liquid is not particularly limited, but is preferably in the range of 0.01% by weight to 10% by weight, more preferably in the range of 0.02% by weight to 7% by weight, and further preferably in the range of 0.025% by weight to 5% by weight.
[0103] Furthermore, in order to further improve the dyeing efficiency, it is preferred to add an iodine compound to the dyeing treatment solution. The iodine compound is a compound containing iodine and an element other than iodine in the molecule. Examples of the iodine compound include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. When an iodine compound is added, its concentration is preferably 0.01% to 10% by weight, and more preferably 0.1% to 5% by weight. Among the iodine compounds, potassium iodide is preferably added.
[0104] When the dyeing liquid 42 contains iodine and an iodine compound, iodine may be the main component of the dyeing liquid (the main component refers to the component with a higher content (weight basis)), or the iodine compound may be the main component of the dyeing liquid. Generally, a dyeing liquid containing more iodine compounds than iodine is used.
[0105] <Cross-linking treatment tank>
[0106] The cross-linking treatment tank 1C is a treatment tank that contains a cross-linking treatment liquid 43. The cross-linking treatment tank 1C cross-links the dyed original film roll 3.
[0107] It should be noted that, although only one cross-linking treatment tank 1C is provided in the example of the figure, two or more cross-linking treatment tanks 1C may be arranged in a row in the moving direction of the original film roll 3 (not shown).
[0108] The cross-linking treatment liquid 43 is a treatment liquid for cross-linking the original film roll 3 to which the aforementioned dichroic substance is adsorbed.
[0109] As the cross-linking treatment liquid 43, a solution containing a boron compound as an effective ingredient can be used. For example, as the cross-linking treatment liquid 43, a solution obtained by dissolving a boron compound in a solvent can be used. As the aforementioned solvent, water is generally used, but an organic solvent compatible with water can also be further added. As boron compounds, boric acid, borax, etc. can be listed. Among them, boric acid is preferably used. As the concentration of the boron compound in the cross-linking treatment liquid, it is not particularly limited, preferably 1% to 10% by weight, more preferably 2% to 7% by weight, and further preferably 2% to 6% by weight. In addition, glyoxal, glutaraldehyde, etc. can be added to the cross-linking treatment liquid as needed.
[0110] Furthermore, since a polarizing film with uniform optical properties can be obtained, an iodine compound is preferably added to the cross-linking treatment solution. As the iodine compound, there is no particular limitation, and the substances exemplified in the above-mentioned dyeing treatment solution can be listed. Among them, potassium iodide is preferred. The concentration of the iodine compound is not particularly limited, preferably 0.05% by weight to 15% by weight, more preferably 0.5% by weight to 8% by weight. When an iodine compound is added, the ratio of the boron compound (preferably boric acid) to the iodine compound (preferably potassium iodide) is preferably in the range of 1:0.1 to 1:6, more preferably 1:0.5 to 1:3.5, and further preferably 1:1 to 1:2.5 by weight.
[0111] When the cross-linking treatment solution 43 contains a boron compound and an iodine compound, the boron compound may be the main component of the solution, or the iodine compound may be the main component of the solution.
[0112] <Stretching treatment tank>
[0113] The stretching treatment tank 1D is a treatment tank that contains a stretching treatment liquid 44. The stretching treatment tank 1D stretches the original film roll 3.
[0114] It should be noted that, although only one stretching treatment tank 1D is provided in the example of the figure, two or more stretching treatment tanks 1D may be arranged in a row in the moving direction of the original film roll 3 (not shown).
[0115] There is no particular limitation on the stretching treatment liquid 44, and for example, a solution containing a boron compound as an active ingredient can be used. As the stretching treatment liquid 44, for example, a solution obtained by dissolving a boron compound and various metal salts, zinc compounds, etc. as required in a solvent can be used. As the aforementioned solvent, water is generally used, but an organic solvent compatible with water can also be further added. As boron compounds, boric acid, borax, etc. can be listed, among which boric acid is preferably used. The concentration of the boron compound in the stretching treatment liquid is not particularly limited, but is preferably 1% to 10% by weight, and more preferably 2% to 7% by weight.
[0116] Furthermore, from the perspective of suppressing the dissolution of iodine adsorbed on the film, the aforementioned stretching treatment liquid preferably contains an iodine compound in addition to the boron compound. The iodine compound is not particularly limited, and the substances exemplified in the aforementioned dyeing treatment liquid can be cited. Among them, potassium iodide is preferred. The concentration of the iodine compound in the stretching treatment liquid is not particularly limited, but is preferably 0.05% by weight to 15% by weight, and more preferably 0.5% by weight to 8% by weight.
[0117] When the stretching treatment liquid 44 contains a boron compound and an iodine compound, the boron compound may be the main component of the solution, or the iodine compound may be the main component of the solution. Generally, a stretching treatment liquid containing more iodine compound than boron compound is used.
[0118] For example, as the stretching treatment liquid 44, a solution containing about 5 wt% of potassium iodide and about 4 wt% of boric acid can be used.
[0119] <Washing treatment tank>
[0120] The washing treatment tank 1E is a treatment tank containing a washing treatment liquid 45. The washing treatment tank 1E washes the original film roll 3 after stretching.
[0121] In addition, although only one washing treatment tank 1E is provided in the example of the figure, two or more washing treatment tanks 1E may be arranged in a row in the moving direction of the original film roll 3 (not shown).
[0122] The cleaning treatment liquid 45 is a treatment liquid for cleaning treatment liquids such as a dyeing treatment liquid and a cross-linking treatment liquid adhering to the original film roll 3 .
[0123] As the cleaning treatment liquid, water such as ion-exchanged water, distilled water, and pure water can be typically used.
[0124] <Others>
[0125] A drying device 21 is provided between the washing treatment tank 1E and the rear roller unit 29. The drying device 21 is provided to dry the original film roll 3.
[0126] It should be noted that, in the example shown in the figure, the manufacturing device 2 has a swelling treatment tank 1A, a dyeing treatment tank 1B, a cross-linking treatment tank 1C, a stretching treatment tank 1D, and a washing treatment tank 1E, but it may not have one or two of the treatment tanks. For example, the manufacturing device 2 may be a device having a swelling treatment tank 1A, a dyeing treatment tank 1B, a cross-linking treatment tank 1C, and a washing treatment tank 1E as treatment tanks, or may be a device having a swelling treatment tank 1A, a dyeing treatment tank 1B, and a cross-linking treatment tank 1C as treatment tanks.
[0127] In addition, the manufacturing apparatus 2 may further include a conditioning treatment tank (not shown).
[0128] The conditioning treatment tank is a treatment tank containing a conditioning treatment liquid. Figure 2 Although not shown in the figure, it is provided between the cross-linking treatment tank 1C and the stretching treatment tank 1D, or between the stretching treatment tank 1D and the washing treatment tank 1E.
[0129] The aforementioned adjustment treatment liquid is a solution for adjusting the hue of the film, and a solution containing an iodine compound as an effective ingredient can be used. For example, as the adjustment treatment liquid, a solution obtained by dissolving an iodine compound in a solvent can be used. The concentration of the iodine compound in the adjustment treatment liquid is not particularly limited, but is preferably 0.5% by weight to 20% by weight, and more preferably 1% by weight to 15% by weight.
[0130] <Method for producing polarizing film>
[0131] Reference Figure 2 The original film roll 3 before treatment is unwound from the front roller portion 28, and the original film roll 3 is transported to the swelling treatment tank 1A by a transport device.
[0132] While the original film roll 3 is conveyed by the guide rollers 25 in the swelling treatment tank 1A, the original film roll 3 is immersed in the swelling treatment liquid 41 to swell the original film roll 3.
[0133] The temperature of the swelling treatment solution 41 is not particularly limited, and is, for example, 20° C. to 45° C., preferably 25° C. to 40° C. The time for immersing the original film roll 3 in the swelling treatment solution 41 is not particularly limited, and is, for example, 5 seconds to 300 seconds, preferably 8 seconds to 240 seconds.
[0134] The original film roll 3 after the swelling step is taken out from the swelling treatment tank 1A, and the original film roll 3 is transported to the dyeing treatment tank 1B.
[0135] While the original film roll 3 is conveyed by the guide rollers 25 in the dyeing treatment tank 1B, the original film roll 3 is immersed in the dyeing treatment liquid 42 to dye the original film roll 3 with the dichroic substance.
[0136] The temperature of the dyeing treatment liquid 42 is not particularly limited, and is, for example, 20° C. to 50° C., preferably 25° C. to 40° C. The time for immersing the original film roll 3 in the dyeing treatment liquid 42 is not particularly limited, and is, for example, 5 seconds to 300 seconds, preferably 8 seconds to 240 seconds.
[0137] The original film roll 3 after the dyeing step is taken out from the dyeing treatment tank 1B, and the original film roll 3 is transported to the cross-linking treatment tank 1C.
[0138] While the original film roll 3 is conveyed by the guide roller 25 of the cross-linking treatment tank 1C, the original film roll 3 is immersed in the cross-linking treatment liquid 43 to cross-link the dichroic substance of the original film roll 3.
[0139] The temperature of the crosslinking treatment solution 43 is not particularly limited, and is, for example, 25° C. or higher, preferably 30° C. to 85° C., and more preferably 40° C. to 70° C. The time for immersing the original film roll 3 in the crosslinking treatment solution 43 is not particularly limited, and is, for example, 5 seconds to 800 seconds, and preferably 6 seconds to 500 seconds.
[0140] The original film roll 3 after the cross-linking step is taken out from the cross-linking treatment tank 1C, and the original film roll 3 is transported to the stretching treatment tank 1D.
[0141] In the stretching treatment liquid 44 of the stretching treatment tank 1D, the film stock roll 3 is stretched while being conveyed by the guide roller 25. The temperature of the stretching treatment liquid 44 is not particularly limited, and is, for example, 40°C to 90°C, preferably 60°C to 90°C or 60°C to 85°C. The stretching ratio can be appropriately set according to the purpose, and the total stretching ratio is, for example, 2 times to 7 times, preferably 4.5 times to 6.8 times. The above-mentioned total stretching ratio refers to the final stretching ratio of the film stock roll 3. The film stock roll 3 may be stretched in at least one tank selected from the swelling treatment tank 1A, the dyeing treatment tank 1B, and the cross-linking treatment tank 1C, or may be stretched only in the stretching treatment tank 1D. The above-mentioned total stretching ratio refers to the ratio when stretching is performed only in the stretching treatment tank 1D, and refers to the sum of their stretching ratios when stretching is also performed in the swelling treatment tank 1A, etc.
[0142] The film stock roll 3 after the stretching step is transported to a conditioning tank as needed and immersed in a conditioning solution. The temperature of the conditioning solution is not particularly limited, and is, for example, 15° C. to 40° C. The time for immersing the film stock roll 3 in the conditioning solution is not particularly limited, and is, for example, 2 seconds to 20 seconds.
[0143] The original film roll 3 after the stretching step or the conditioning step is transported to the cleaning treatment tank 1E and is immersed in the cleaning treatment liquid 45 to thereby clean the original film roll 3 .
[0144] The temperature of the cleaning solution 45 is, for example, 5° C. to 50° C., or preferably 10° C. to 45° C. The cleaning time is, for example, 1 second to 300 seconds, or preferably 3 seconds to 240 seconds.
[0145] The original film roll 3 after the washing step is dried by the drying device 21 as needed, thereby obtaining the polarizing film 5 . The produced polarizing film 5 is wound up by the rear roll unit 29 .
[0146] The processing tank 1 for manufacturing polarizing film of the present invention is provided with a coating layer 12 having an elongation of 150% or more on the inner surface of the metal tank body 11, thereby preventing the tank body 11 from being corroded by the processing liquid. In detail, since the corrosion-resistant coating layer 12 is provided on the inner surface of the tank body 11, the processing liquid does not contact the tank body 11, thereby preventing the tank body 11 from being corroded. In addition, if the processing tank 1 is used for a long time, the metal tank body 11 will be deformed. In particular, if a processing liquid at a relatively high temperature (for example, above 40°C) is contained in the processing tank, the metal constituting the tank body 11 will be easily deformed by thermal expansion. In this regard, in the present invention, since the thermal expansion coefficient of the tank body 11 is 10×10 -6 / ℃~24×10 -6 The coating layer 12 with a temperature of 0.17°C covers the inner surface of the tank body 11, so the coating layer 12 flexibly expands following the thermal expansion of the tank body 11. Therefore, the coating layer 12 is not easily cracked or peeled off due to deformation of the tank body 11, and the tank body 11 can be prevented from being corroded by the processing liquid.
[0147] In the past, when cracks or peeling occurred in the processing tank for manufacturing polarizing film, it was considered that the cause was aging, and the processing tank was repaired or replaced. In this regard, the present inventors have explored the causes of cracks or peeling of the existing coating layer and found that it is due to the thermal expansion of the metal tank body and the followability of the coating layer to the expansion. In addition, the present inventors combined the coating material that easily follows the expansion (deformation) of the tank body with the tank body, thereby providing a processing tank that can effectively suppress cracks in the coating layer.
[0148] [Applications of polarizing films, etc.]
[0149] The polarizing film of the present invention can be used, for example, in lenses of sunglasses, dimming windows, image display devices such as liquid crystal displays, and the like.
[0150] The polarizing film of the present invention can also be used as a polarizing plate by laminating a protective film on one or both sides thereof. When used as a polarizing plate, a retardation film can be further laminated.
[0151] Example
[0152] Hereinafter, the present invention will be described in further detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0153] [Material for forming the groove body]
[0154] Stainless steel plate
[0155] SUS304 stainless steel plate with a length × width × thickness = 100 mm × 50 mm × 5 mm. This SUS304 is a JIS standard product with a linear expansion coefficient of 17.3 × 10 -6 / ℃.
[0156] [Coating material]
[0157] Polyurea resin (1)
[0158] Trade name: "Nukote ST" (manufacturer: NUKOTE Co., Ltd., seller: Kanemori Fujihei Shoji Co., Ltd.) Elongation: 400%.
[0159] Polyurea resin (2)
[0160] Trade name: "Nukote HT" (manufacturer: NUKOTE Co., Ltd., seller: Kanemori Fujihei Shoji Co., Ltd.) Elongation: 375%.
[0161] Polyurea resin (3)
[0162] Trade name: "Nukote CG" (manufacturer: NUKOTE Co., Ltd., seller: Kanemori Fujihei Shoji Co., Ltd.) Elongation: 175%.
[0163] Polyurea resin (4)
[0164] Trade name: "Nukote XT-Plus" (manufacturer: NUKOTE, sold by: Kanemori Fujihei Shoji Co., Ltd.) Elongation: 50%.
[0165] The polyurea resins (1) to (3) are two-component curing types of an agent A containing an isocyanate as a main component and an agent B containing an amine compound as a main component.
[0166] Butyl rubber
[0167] Trade name: "Butyl rubber" (manufacturer: Meiwa Rubber Industries, Ltd.) Elongation: 360%.
[0168] ·Vinyl chloride resin
[0169] Trade name: "vinyl chloride" (manufacturer: Shin-Etsu Chemical Co., Ltd.) Elongation: 60%.
[0170] ·FRP (Fiber Reinforced Plastic)
[0171] Trade name: "NEOPOL 8411LH" (manufacturer: Japan U-Pica Company Ltd.). Elongation: 2%.
[0172] Ceramic / metal composite polymer
[0173] Trade name: "Nukote Chemshield" (manufacturer: NUKOTE Co., Ltd., distributor: Kanemori Tohei Shoji Co., Ltd.) Elongation: 5%.
[0174] It should be noted that the elongation of polyurea resins (1) to (4) is measured by a tensile test in accordance with ASTM-D412. The elongation of butyl rubber is measured by a tensile test in accordance with JIS K6251:2017. The elongation of vinyl chloride resin is measured by a tensile test in accordance with ASTM-D638. The elongation of FRP (fiber reinforced resin) is measured by a tensile test in accordance with JIS K7161-1:2014. The elongation of ceramic / metal composite polymer is measured by a tensile test in accordance with ASTM-D638.
[0175] [Example 1]
[0176] The polyurea resin (1) was applied to cover the entire surface of the stainless steel plate and cured to prepare a sample sheet in which the entire surface of the stainless steel plate was covered with a 3 mm thick coating layer made of the polyurea resin (1).
[0177] [Example 2]
[0178] A sample sheet of Example 2 was prepared in the same manner as in Example 1 except that the polyurea resin (2) was used instead of the polyurea resin (1).
[0179] [Example 3]
[0180] A sample sheet of Example 3 was prepared in the same manner as in Example 1 except that the polyurea resin (3) was used instead of the polyurea resin (1).
[0181] [Example 4]
[0182] A sample sheet of Example 4 was prepared in the same manner as in Example 1 except that butyl rubber was used instead of the polyurea resin (1).
[0183] [Comparative Examples 1 to 4]
[0184] Sample sheets of Comparative Examples 1 to 4 were prepared in the same manner as in Example 1 except that the covering materials shown in Table 1 were used instead of the polyurea resin (1).
[0185] [Table 1]
[0186] Covering material Elongation(%) Test results Example 1 Polyurea resin(1) 400 AAA Example 2 Polyurea resin(2) 375 AAA Example 3 Polyurea resin(3) 175 AA Example 4 Butyl rubber 360 AA Comparative Example 1 Polyurea resin(4) 50 B Comparative Example 2 Vinyl chloride resin 60 B Comparative Example 3 FRP 2 B Comparative Example 4 Composite polymer 5 B
[0187] [Durability test]
[0188] Each sample piece of Examples 1 to 4 and Comparative Examples 1 to 4 was immersed in an aqueous solution containing boric acid and potassium iodide (boric acid concentration of about 7 wt %, potassium iodide concentration of about 8%) maintained at a liquid temperature of 70° C. for one month.
[0189] After being immersed for one month, each sample piece was taken out from the solution, and the state of the coating layer was visually observed. The results are shown in Table 1.
[0190] In the test results in Table 1, "AAA" indicates that the coating layer did not crack or peel and was not corroded, "AA" indicates that the coating layer did not crack or peel but the surface of the coating layer was slightly corroded, and "B" indicates that cracks or peeling occurred in at least one location in the coating layer.
[0191] The coating layers of Examples 1 to 4 formed by coating materials having an elongation of 175% or more did not crack or peel off, while the coating layers of Comparative Examples 1 to 4 formed by coating materials having an elongation of 60% or less cracked or peeled off. It can be said that by using a coating material having an elongation of about 150% or more, a coating layer that is not prone to cracking or peeling can be formed. In addition, according to the comparison between Examples 1 and 2 and Examples 3 and 4, it can be seen that by using a polyurea resin having an elongation of 350% or more, a coating layer that is not prone to cracking or peeling off for a long time and is not easily corroded by the treatment liquid can be formed.
Claims
1. A processing tank for manufacturing polarizing film, It is a processing tank for containing a processing liquid used when making a polarizing film from a film original roll, wherein: The processing tank has a metal tank body and a coating layer covering the inner surface of the tank body. The coating layer is formed of a coating material having an elongation of 150% to 500%.
2. The processing tank for producing polarizing film according to claim 1, wherein: The coating layer is formed of a coating material having an elongation of 350% to 450%.
3. The processing tank for producing polarizing film according to claim 1 or 2, wherein: The thermal expansion coefficient of the tank body is 10×10 -6 / ℃~24×10 -6 / ℃.
4. The processing tank for producing a polarizing film according to claim 1 or 2, wherein: The covering material contains a polyurea resin.
5. The processing tank for producing polarizing film according to claim 1 or 2, wherein: The coating layer has a thickness of 1.0 mm or more.
6. The processing tank for producing a polarizing film according to claim 1 or 2, wherein: The tank body is formed of stainless steel. 7 . The treatment tank for producing a polarizing film according to claim 1 , which is at least one of a cross-linking treatment tank for cross-linking an original film roll and a stretching treatment tank for stretching an original film roll.
8. A manufacturing device for a polarizing film, comprising: The treatment tank according to any one of claims 1 to 7; a treatment liquid contained in the treatment tank; and, A conveying device for conveying the original film roll and immersing it in the treatment liquid in the treatment tank.
9. The manufacturing device of the polarizing film according to claim 8, wherein: The processing liquid contains at least one of an iodine compound and a boron compound.
10. The manufacturing device of the polarizing film according to claim 8 or 9, wherein: The temperature of the treatment liquid is above 40°C.